Re: [MW:27557] Re: If a welder is qualified with SS (Stainless Steel) GTAW, He can weld CS Carbon steel GTAW?

For welder A no is not essential??

On Sat 24 Mar, 2018 5:12 pm Vairamuthu, <vaira.muthu.78@gmail.com> wrote:

As Mr. Chandra is clearly said the welder can't weld in CS as code very clear on this and very nicely explained by Chandra Ji. which is copied below. 

Dear Team,
 Both the carbon and stainless steel filler metals 
Fno. is 6.
Refer QW-404.15 (A change from one F-no in table
Qw-432 to any F-number or to any other filler
metal, except as permitted in Qw-433.
Qw-433 table says qualified with any F.no6 qualified 
For all F-No 6 [refer note1]
Note1 says: deposited wels metal made using a 
bare rod not covered by an SFA specification
but which conforms to an analysis listed in 
Table QW-442 shall be considered to be classified
As F-no 6.

Means carbon steel F.No 6 (but A.No is 1)
 Stainless steel F.No 6 (but A.No is 8)

So, even F.no same but weld metal analysis is
different. So he was not qualified to weld stainless

Best Regards,
Chandra



On Saturday, February 24, 2018 at 1:03:47 PM UTC+3, PK wrote:
Dear Sir,

If a welder is qualified with SS (Stainless Steel) GTAW,  He can weld CS Carbon steel GTAW? Need code Referance...

Thanks.
PKM

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...