Re: [MW:27494] Impact Test for Procedure Qualification

The design Code (B31.3 in this case   takes precedence over Section IX, when there is  a difference. 


On Mon, 12 Mar 2018 at 08:35, Ramesh <rameshkannandevaraj@gmail.com> wrote:
Hi Jibin & All

This is my first Entry to this Group... if any mistakes correct me.. Thanks


As a first step, refer Table QW-451.1 in ASME Sec IX for PQR thickness limits. 

Based on some Essential / supplementary variables this Minimum or Maximum thickness will vary from this table.

For example, refer QW-256 -GTAW welding variable table. u can see QW403.6 , QW 407.4  i.e T limits row and study relevant QW clause which is self explanatory

Your case

Q1) What will be the thickness range qualified is it 10.97 to 16.97 or 5 mm to 16.97 or 5 mm to 21.94.

Since your PQR have impact requirement i.e supplementary variable requirements , Your PQR thickness range qualified is 10.97 to 21.94

Q2) If i need to qualify a WPS with Thk ranges 5 mm to 25mm which thickness need to be selected .

Qualify one PQR (1) with 6 mm thick, this will qualify 3 to 12 mm thk

Qualify other PQR (2) with 12 mm thick , this will qualify 12 to 24 mm thk 

Qualify other PQR (3) with 25 mm thick, thick will qualify 16 to 50 mm thk

So you will have WPS combining all PQRs with 3 to 50 mm which almost covers all your Fabrication requirement for CS pipes.

Hope this helps you...

Thanks and Regards,


Rameshkannan Devaraj





On Sun, Mar 11, 2018 at 5:58 PM, Babur Khan <mbabur.bwp@gmail.com> wrote:
Dear sir,
As per ASME Sec ix QW-403.6 
Min. T (10.97) mac 2T.
Regards,
M. Babur Khan Lashari

Sent from my iPhone

On 11 Mar 2018, at 12:58 PM, Raghuram Bathula <raghurambathula@gmail.com> wrote:




On Sun, 11 Mar 2018 at 13:46, Jibin Philip <jibinphilip123@gmail.com> wrote:
Dear All , 

Spec - ASME B31.3 (Ed : 2016)  & Sec IX (Ed : 2017) ,

For PQR-A106 GR B -  i have taken 6" pipe Thk - 10.97mm - with impact test

Q1) What will be the thickness range qualified is it 10.97 to 16.97 or 5 mm to 16.97 or 5 mm to 21.94.
 
10.97 to 16.97 
Q2) If i need to qualify a WPS with Thk ranges 5 mm to 25mm which thickness need to be selected .
you need to have multiple test coupons 
Regards , 

Jibin 


--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

[MW:30043] Weep hole

If weep hole is not provided in dummy pipe before welding What will happen??? -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/da251ee6-fa7f-4851-b876-cdb3834ae341%40googlegroups.com .