Re: [MW:15055] 14919] Stress relieving Rejected for 5 min less soaking time.

this is valid for qualification purposes and not for fabrication purposes. You have to perform a second PWHT cycle
Best regards
Dr Georgios Dilintas
Authorized Nuclear Inspector
Authorized Inspector Supervisor
HBS Regional Technical Manager


  From: "sachin sankhe" [sachin.sankhe@rediffmail.com]
  Sent: 07/08/2012 17:34 GMT
  To: "materials-welding@googlegroups.com" <materials-welding@googlegroups.com>
  Subject: Re: [MW:15039]  14919] Stress relieving Rejected for 5 min less soaking time.


Hi Friends

ASME SEC IX gives relaxation on soaking time i.e atleast 80% of that required on production joint

Regards
Sachin.Sankhe




From: "pgoswami" <pgoswami@quickclic.net>
Sent: Wed, 25 Jul 2012 17:44:39
To: <materials-welding@googlegroups.com>
Subject: Re: [MW:14949] 14919] Stress relieving Rejected for 5 min less soaking time.
Harish/Mohd,
 
I am not trying to act as moderator.
 
Looking at the problem, a separate simulation may be as time consuming as the original HT. Code is a law, with engineering judgments. Hence the inspector has the rights to declare that the original HT was inadequate. The simplest solution what looks to me is to perform additional SR for 15-20 mins and satisfy code requirements.
 
PWHT time is all cumulative , and there no restriction form ASME code.
 
Thanks.
 

Pradip Goswami,P.Eng.IWE

Welding & Metallurgical Specialist

Ontario, Canada.

Email-pgoswami@sympatico.ca,

pgoswami@quickclic.net

 


From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of Harish Kannepalli
Sent: Monday, July 23, 2012 11:58 AM
To: materials-welding@googlegroups.com
Subject: Re: [MW:14942] RE: 14919] Stress relieving Rejected for 5 min less soaking time.

You can propose the following to your client:
            Perform Simulation on separate coupon, check the mechanical & metallurgical properties. If they meet the code requirements, it may be acceptable. After all, code is made by humans for humans.

2012/7/23 John Henning <jhenning@deltak.com>

Most common materials require 1 hour/25mm or 60minutes/25mm and I assume you are working with one of these materials.  Then, for a 40mm thick material the required minimum soak time is (40mm)*(60min.)/(25mm) = 96 minutes

 

You don't meet Code required minimum soak time.  Your soak time must exceed the minimum time.  Therefore, your pipe weld is unacceptable.  No discussion – it is clearly unacceptable in its present condition.

 

John A. Henning

Welding & Materials

 

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of mohd
Sent: Saturday, July 21, 2012 1:52 AM
To: materials-welding@googlegroups.com
Subject: [MW:14919] Stress relieving Rejected for 5 min less soaking time.

 

Dear expert,

 

As per ASME 8-1-UCS-56

 

We have done SR for our 40mm thk-30" pipe joint.

 

but unfortunetly, soaking time was just short by 5min.Now our client/PMC both are not agree to release.

 

Required time : 1hr.15min

Actual Time : 1hr.10min

 

It is acceptable OR could you share any technical view to convince client?

 

regards,

mohd.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.


______________________________________________________________________
The information in this email is confidential, and is intended solely for the addressee(s). If you are not the intended recipient of this email please let us know by reply and then delete it from your system; you should not copy this message or disclose its contents to anyone. The internet can not guarantee the integrity of this message. HAMON (and its subsidiaries) shall (will) not therefore be liable for the message if modified.
______________________________________________________________________

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.



--
regards,
Harish.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.


Follow Rediff Deal ho jaye! to get exciting offers in your city everyday.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
 
 
~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~
NOTICE: This message contains information which is confidential and the copyright of our company or a third party. If you are not the intended recipient of this message please delete it and destroy all copies. If you
are the intended recipient of this message you should not disclose or distribute this message to third parties without the consent of our company. Our company does not represent, warrant and/or guarantee that the integrity of this message has been maintained nor that the communication is free of virus, interception or interference. The liability of our company is limited by our General Conditions of Services.
Nota : Ce message contient des informations confidentielles propriété de notre société et/ou d'un tiers. Si vous n'êtes pas parmi les destinataires désignés de ce message, merci de l'effacer ainsi que toutes ses copies. Si vous êtes parmi les destinataires désignés de ce message, prière de ne pas le divulguer ni de le transmettre à des tiers sans l'accord de notre société. Notre société ne peut garantir que l'intégrité de ce message a été préservée ni que la présente communication est sans virus, interception ou interférence. La responsabilité de notre société est limitée par nos Conditions Générales de Services.
~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
 
 

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...