Skip to main content

Re: [MW:4990] API 5L X85 -CVN Requirements

Mr. K. Babu:
 
API 5L ,ed. 44, does not request longitudinal CVN test, because due to rolling process for plate production for seam weld pipe or seamless pipe, the grain orientation of the microstructure has the lowest  fracture toughness values  transverse to pipe axis. Therefore, CVN spicemens must be taken transverse to the pipe axis based on the fact that this is the most unfavorable spicemen orientation to obtain the minimum requested absorbed energy values
On the other hand, X85 grade is an intermediate grade agreed for production between purchaser and manufacture
According to table 8 of API 5L, for body full size absorb energy the values for X85 grade can be interpolated according to values for grades X80 and X90 which is 30 ft-lb for pipe diameters from 20 to 36 inches and for test temp of 0°C (32°F), or lower temperature if agreed.
 
For CVN test for seam weld and H.A.Z., according to 9.8.3, the absorb energy value is also 30 ft-lb at 0°C (32°F), or lower temperature if agreed.
 
Carlos Quintini
Quintini Consultores C.A.
Venezuela

2010/4/28 Kathalingam Babu <kathalingam.qaqc@ppl.com.sg>
There is an intermediate grade called API 5L X85 , it is commonly used in offshore industries.
 
Might be added in next edition of API 5L Spec.
 
Sent: Wednesday, April 28, 2010 4:17 PM
Subject: RE: [MW:4973] API 5L X85 -CVN Requirements

I heard that 44th edition of API 5L has 3 new grades X90, X100 and X120.
what is X85? CVN is mandatory for all PSL2 pipes, refer para 6.2.5.2


From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of Kathalingam Babu
Sent: Tuesday, April 27, 2010 3:53 PM
To: materials-welding@googlegroups.com
Subject: [MW:4966] API 5L X85 -CVN Requirements

Gents,
 
Pls tell me, what is the CVN (Longitudinal) Requirements for the API 5L X85 (19 mm thick) ?
 
Thanks & Regards,
 
K.Babu


--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...