Re: [MW:4955] Acceptability of Inconel pipe.

The specification calls for testing at pressure which shall create hoop stress equivalent to the material SMYS (30 kpsi in this case).
 
To create this hoop stress, the pipe of this schedule need to be tested at 7492 psi only. (formula P = 2xsxt/D)
 
Sanjeevan
 
----- Original Message -----
Sent: Sunday, April 25, 2010 6:14 PM
Subject: [MW:4952] Acceptability of Inconel pipe.



Hi Dear friends,


Please anybody help me for the below,

For our new ASME job, we need inconel materials and we are not so familiar with this. We checked three test certificate from different supplier for inconel 625 (3" Sch160, smls) pipe and here all hydrostatic test is conducted at 8829 psi. But as per ASME Section II, Part B, ED 07, Add08 hydrostatic test pressure shall be 30000psi for SB444, UNS N06625, Gr.1 material. So please advise me that anyway we can accept material having the preesure test value of 8829 psi.

And also please explain what is allowable fiber stress and from where we get values of allowable fibre stress for this material.



Thanks & Regards,

SMRUTHI MOHAN
ENGINEER - MATERIALS
QICL, FUJAIRAH

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...