Skip to main content

Re: [MW:22023] Max. temp. attainable by CS tubes to avoid creep rupture

Hi everyone,though therotically Maximum Temperature limit of C.S is 425 degree celcius but you refer some practical standard of API it will allow use of c.s. above 425 degree celcius. any how its tube so obiviously threre will be less welding so the rate of carbide formation will be less. i dont think so it will be issue for 1 hour

On Tue, Sep 30, 2014 at 5:15 PM, pgoswami <pgoswami@quickclic.net> wrote:
Hi Jignesh and Dr Dilintas,
 
A short note on this scenario, from Utility Operators point of view.
C.S will be pushed well above the upper limit and cause overheating of SA 106 GrB. Reason excessively higher temperature(well above design limits) plus dry(no flow condition).
 
It would advisable to switch to Cr-Mo steel for better design, and avoid premature failure. FEA is good for all other scenario, but Creep is totally unpredictable.
 
Thanks.
 
Pradip Goswami, P.Eng,IWE
Welding & Metallurgical Specialist
Ontario, Canada
 


From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of george.dilintas@gr.bureauveritas.com
Sent: Tuesday, September 30, 2014 4:29 AM
To: materials-welding@googlegroups.com
Subject: Re: [MW:22020] Max. temp. attainable by CS tubes to avoid creep rupture

The max temp. for SA-106 GrB is 800 deg F (as indicated by ASME B31.1).
Your temperature is close to this limit.
However, creep is not only a function of time. It is a function also of the load (pressure or other).
So I would suggest that you carry a static calculation and you compare the resulting stress with the allowable stress at 800 degF (for SA-106GrB, this is 10,8 ksi).
If you are below you have not to worry about.
Otherwise you will need to perform FEA with non linear Finite Elements simulating creep

    best regards

    Dr. Georgios Dilintas

    Authorized Nuclear Inspector
    Authorized Inspector Supervisor


    I&F REGIONAL TECHNICAL MANAGER
    BUREAU VERITAS HELLAS

    Tel: +30 210 40 63 113/4
    Fax: +30 210 40 63 118
    Cell: +30 69 44 64 62 04
    (See attached file: Dilintas_George.vcf)

Jignesh Desai ---30/09/2014 10:52:54---Design Code : ASME Sec I, API 560 & API 530 Service: Non Corrosive.

From: Jignesh Desai <jignesh.desai.met@gmail.com>
To: materials-welding@googlegroups.com
Date: 30/09/2014 10:52
Subject: [MW:22019] Max. temp. attainable by CS tubes to avoid creep rupture
Sent by: materials-welding@googlegroups.com




Design Code : ASME Sec I, API 560 & API 530
Service: Non Corrosive.


We have CS tubes in the convection section (BFW service) of furnace and we are planning to operate during the emergency shut down (plant black out) for short duration of about an hour at higher temperature then the design temp.  (425° C).
At this short duration of time the water tubes is going to see the no BFW flow condition (DRY).

Query: What is the max. temperature attainable (intermittent - 01 hour) by CS tubes (to avoid creep rupture). How much the temperature above the design temperature (425° C) can the CS tube be pushed for this short operation of time (01 hour)?

Regds/Jignesh

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at
http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm

The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to
materials-welding+unsubscribe@googlegroups.com.
For more options, visit
https://groups.google.com/d/optout.

This message contains confidential information. To know more, please click on the following link: http://disclaimer.bureauveritas.com

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/d/optout.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/d/optout.



--
Thanks And Regards,
Nitin R. Patil
B.E.(Mechanical)
Mobile No-8087065569

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/d/optout.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...