USE 98%ARGON + 2% O2 FOR SS SOLID WIRE

THANKS & BEST REGARDS
KG.PANDITHAN, AWS-CWI, CSWIP 3.1
CONSULTANT-WELDING & QUALITY

On Wed, Sep 24, 2014 at 10:56 AM, Vadivel Mahadevan <vadivelmahadev@gmail.com> wrote:
Dear Experts,
Thanks for your view.
 
Mr. Pradip,
I am using Sheilding medium - 80% Argon & 20% CO2
Welding position is 2FR and the fillet weld arrangement is shown in the attached file.
Welding is done on fully mechanised(automatic) machine.
I have done a Pipe to plate joint in which I have used only 16-18V and the pipe schedule is Sch.80-2"pipe.
 
Mr. Sayee,
As you said, I experienced the same in CS and SS material.
I didnt come across LOF in CS, whereas in SS it is so.
 
Experts,
Can you please tell me the basic difference an dhow to identify Short circuiting & spray transfer mode. How can I switch over.
Regards
Vadivel. M

On Wednesday, September 24, 2014 9:08:25 AM UTC+5:30, Sayee Raghunathan wrote:
Vadivel

Shielding gas and inductance are most important factors without disregarding all others that Goswami metioned in his email.

Note that due to sluggish nature of ss weld pool due to increased Ni and Cr contents in general implies lower weld pool fluidity and higher susceptibility for LOF than c-steel welding for example. Hence, check if these two (inductance and shielding gas with 2%o2 or Co2, more preferably a He gas mix giving hotter arc and correct weld bead profile) are correctly being applied before investigating other factors.

Regards

Sayee

On Tuesday, 23 September 2014, pgoswami <pgos...@quickclic.net> wrote:
Hi Vadivel,
 
What're the  welding parameters (including shielding gas) being used??. What's the welding position? Are the welders' qualified for all position welding?
 
There're many  subtle variables for GMAW, which play important roles between, procedure qualification and production welds.
 
Please read this attachment to understand the basic. GMAW-S could be often problematic, especially for positional welding and the shielding gases involved. GMAW-P could be a better option in many instances. Modern machines have features like STT or Miller -RMD, which offers much better control. It's worth looking at , if you have such machines at your works.
 
GMAW is an excellent process, but takes time to produce results, which temps the fabricators to switch to FCAW. However it's not worth giving up at all.
 
Thanks.
 
 
Pradip Goswami, P.Eng,IWE
Welding & Metallurgical Specialist
Ontario, Canada
 


From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of Vadivel Mahadevan
Sent: Monday, September 22, 2014 8:28 AM
To: materials-welding@googlegroups.com
Subject: Re: [MW:21970] Lack of fusion in production welding - GMAW !!!

Hello Mr. George,
My LOF is intermittent in majority of the jobs. However in fewer bodies it is continous. I can say 85:15 ratio of the Leaked welds
Regards
Vadivel. M

On Saturday, September 20, 2014 4:10:26 PM UTC+5:30, George Dilintas wrote:

Your LOF is intermittent of continuous?
Best regards
Dr Georgios Dilintas
Authorized Nuclear Inspector
Authorized Inspector Supervisor
HBS Regional Technical Manager


  From: Vadivel Mahadevan [vadivel...@gmail.com]
  Sent: 09/20/2014 02:19 AM MST
  To: material...@googlegroups.com
  Subject: [MW:21945] Lack of fusion in production welding - GMAW !!!


Dear Experts,
 
I face Lack of fusion problem in GMAW process in the production weld often.
WPS qualified on short circuiting mode as the torch is designed to the same.
But when I use the same current and voltage I come across Lack of fusion
The wire I use is ER316L of 1.2mm dia.Bare wire , volt not more than 19V.
 
Now I started using 23 to 26V(Spray transfer mode volt range) to overcome my issue.
Can you suggest what are the parameters I need to control to get a sound weld in the short circuiting mode.
 
Regards
Vadivel. M
07829007400

--
To post to this group, send email to material...@googlegroups.com
To unsubscribe from this group, send email to materials-weld...@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
For more options, visit https://groups.google.com/d/optout.
This message contains confidential information. To know more, please click on the following link: http://disclaimer.bureauveritas.com

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/d/optout.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/d/optout.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/d/optout.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/d/optout.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...