Skip to main content

Re: [MW:21993] Boiler Weld Repair

BEGIN:VCARD
X-LOTUS-CHARSET:UTF-8
VERSION:3.0
PRODID:-//Lotus Development Corporation//NONSGML Notes 8.5.2//EN_C
FN:George H Dilintas/GRC/VERITAS
N:Dilintas;George;;;
ADR;TYPE=WORK;TYPE=PREF:PIRAEUS;;23\, Etolikoy Str.;PIRAEUS;;185 45
;GREECE
ADR;TYPE=HOME;TYPE=PREF:;;19-21 B. Laskou str.;Athens;Attika;11 633
;Greece
TEL;TYPE=HOME:+30-1-7667 197
TEL;TYPE=WORK:+30-210-40 63 113
TEL;TYPE=HOME;TYPE=FAX:+30 - 1 - 7667 197
TEL;TYPE=WORK;TYPE=FAX:+30-210-40 63 118
TEL;TYPE=CELL:+30 -69 44-64 62 04
EMAIL;TYPE=WORK;TYPE=PREF;TYPE=INTERNET
:george.dilintas@gr.bureauveritas.com
ORG:Bureau Veritas;Industry
REV:20131201T024559Z
END:VCARD

I suppose that this is a Fire Tube  Boiler still under manufacturing process.
I assume that the pin holes have been detected on the weld attaching the furnace to the tubesheet.

I assume also that the pin-holes have been detected by means of PT.
Well, Section I does not formally require an inspection by PT at this area. This is not a joint like those addressed in PG-93.2.

If above assumptions are true, you have performed an inspection beyond the Code requirements.
However, since you have done this, you have to look in A-260 for the acceptance criteria (unless they are through pin-holes which will cause leakage)  and then you have to act as required by PG-90.1.10

    best regards

    Dr. Georgios Dilintas

    Authorized Nuclear Inspector
    Authorized Inspector Supervisor


    I&F REGIONAL TECHNICAL MANAGER
    BUREAU VERITAS HELLAS

    Tel: +30 210 40 63 113/4
    Fax: +30 210 40 63 118
    Cell: +30 69 44 64 62 04
    (See attached file: Dilintas_George.vcf)

gunawan refiadi ---24/09/2014 12:37:38---Dear Dr. Georgios Dilintas, I have some pinhole defect on boiler weld circumference (file attached).

From: gunawan refiadi <g4refiadi@gmail.com>
To: materials-welding@googlegroups.com
Date: 24/09/2014 12:37
Subject: [MW:21992] Boiler Weld Repair
Sent by: materials-welding@googlegroups.com




Dear Dr. Georgios Dilintas,

I have some pinhole defect on boiler weld circumference (file attached).
Is there any requirement to repair this defects ?

B.Regards,

Gunawan

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at
http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm

The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to
materials-welding+unsubscribe@googlegroups.com.
For more options, visit
https://groups.google.com/d/optout.[attachment "Lokasi pinhole-1.jpg" deleted by George H Dilintas/GRC/VERITAS] [attachment "Lokasi pinhole-2.jpg" deleted by George H Dilintas/GRC/VERITAS] [attachment "Lokasi pinhole-3.jpg" deleted by George H Dilintas/GRC/VERITAS]

This message contains confidential information. To know more, please click on the following link: http://disclaimer.bureauveritas.com

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...