Dear Sir

Actually this material is for Piling work. We are constructing a new
jetty . Steel Pile material is API - 5 L PSL - 2 / Grade X-65 . Pile
size OD - 1219mm and wall thickness - 22.22mm and also other size OD -
914mm and wall thickness - 22.22mm.

Now I want make a WPS by carrying out PQR . So I am searching based on
the sample pipe's MTC. The reading I have given is replica of MTC and
the is certified by Lloyds Surveyor too.

Now please tell me the correct welding electrode for SMAW and wire and
flux for SAW process. As per API 5L PSL 2 / Grade 65. the requirement -

X 65 - YS - 448 MPa. TS - 531 MPa. EL% - 23 - Impact at 0 deg.C
27 Joules. C - 0.22 Mn - 1.45 P- 0.025
S- 0.015 Ti - 0.06


Approved brands electrodes - ESAB and OERLIKON from these consumables
shall be selected.

While testing PQR it should not fail.

Expecting your mail shortly.

Thanking You.

With Regards,

Muthu Barathi P


On Fri, 28 Jan 2011 03:28:26 +0530 wrote
>


@font-face {
font-family: Tahoma;
}
@font-face {
font-family: Verdana;
}
@page Section1 {size: 595.45pt 841.7pt; margin: .1in .6in 0in .5in; }
P.MsoNormal {
MARGIN: 0in 0in 0pt; FONT-FAMILY: "Times New Roman"; FONT-SIZE:
12pt
}
LI.MsoNormal {
MARGIN: 0in 0in 0pt; FONT-FAMILY: "Times New Roman"; FONT-SIZE:
12pt
}
DIV.MsoNormal {
MARGIN: 0in 0in 0pt; FONT-FAMILY: "Times New Roman"; FONT-SIZE:
12pt
}
A:link {
COLOR: blue; TEXT-DECORATION: underline
}
SPAN.MsoHyperlink {
COLOR: blue; TEXT-DECORATION: underline
}
A:visited {
COLOR: blue; TEXT-DECORATION: underline
}
SPAN.MsoHyperlinkFollowed {
COLOR: blue; TEXT-DECORATION: underline
}
P {
FONT-FAMILY: "Times New Roman"; MARGIN-LEFT: 0in; FONT-SIZE:
12pt; MARGIN-RIGHT: 0in; mso-margin-top-alt: auto; mso-margin-bottom-
alt: auto
}
SPAN.EmailStyle18 {
FONT-FAMILY: Arial; COLOR: navy; mso-style-type: personal-reply
}
DIV.Section1 {
page: Section1
}



Mr. Muthu,

What's the applicable specification for this material,
ASTM/ASME/EN or any proprietary grade for any client or any vendor's
specification.The elongation and impact properties asked are highly
un-realistic. You never get a Carbon or Low Alloy steel with 46%
elongation
requirement, also, impact requirement is extremely high.

I would say, if you have any design paper work, which
indicates the grade or heat treatment of this steel the correct AWS
type of
welding consumables, SAW wire+flux specification etc could be worked
out.
Otherwise YOU SHOULD NEVER CHOOSE WELDING CONSUMABLES BASED ON THE
CHEMICAL
COMPOSITION ALONE.

Thanks.


Pradip Goswami,P.Eng.IWE
Welding & Metallurgical Specialist
& Consultant
Ontario, Canada.
Email-pgoswami@sympatico.ca,
pgoswami@quickclic.net

>


From: materials-welding@googlegroups.com
[mailto:materials-welding@googlegroups.com] On Behalf Of Pablo J
Acelajado
>Sent: Thursday, January 27, 2011 10:08 AM
>To:
materials-welding@googlegroups.com
>Subject: RE: [MW:9529] Requirement
of suitable welding consumables SAW and SMAW
>
>




January 27,
2011

Hello there!

This material is very strong one. I think
the welding consumable suppliers can best answer this question.

My understanding is that the percentage
elongationis not required for the weld.
Thank you.

Best regards.
PJA




From:
materials-welding@googlegroups.com
[mailto:materials-welding@googlegroups.com] On Behalf Of Kathalingam
Babu
>Sent: Thursday, January 27, 2011 1:10
PM
>To: materials-welding@googlegroups.com
>Subject: Re: [MW:9526] Requirement of
suitable welding consumables SAW and SMAW


Hi



The elongation requirement is very stringent, it is very
difficult to meet 46%, you have consult with the specific consumable
suppliers
to get 46%



Thanks & Regards,



K. Babu


>----- Original Message -----



From: muthu barathi


To: materials-welding@googlegroups.com


Sent: Thursday,
January 27, 2011 4:36 PM

Subject: [MW:9523]
Requirement of suitable welding consumables SAW and
SMAW


Hi Friends,
>
>Let me get your expertise of
selection of welding consumables in this
>regard.
>
>The base material
Chemical properties as given under (%):
>
>C - 0.066
>Si - 0.26
>Mn -
1.55
>P - 0.014
>S - 0.004
>Al - 0.046
>Cr - 0.186
>Ni - 0.015
>Mo
- 0.002
>Cu - 0.020
>V - 0.057
>Nb - 0.065
>Ti - 0.020
>N -
0.007
>B - 0.00025
>Ca - 0.0025
>CE - 0.371
>
>MECHANICAL
PROPERTIES
>YIELD STRENGTH - 516 MPa
>TENSILE STRENGTH - 625
MPa.
>ELONG % - 46
>IMOPACT
- (-) 10 DEGREE C - 250 JOULES
>
>NOW PLEASE TELL ME, WHICH
ELECTRODE FOR SMAW (BRAMDS ESAB, OERLIKON)
>AND SAW - FLUX AND WIRE WILL
SUIT AND PASS PQR TEST FOR PREPARATION OF
>WPS?
>
>PLEASE
HELP.
>THANKING YOU.
>
>
>
>Dear
Sir,
>
>
>
>
>
>Thanking You,
>
>Honesty is the best
Policy
>
>With Warm Regards,
>
>Muthu Barathi P
>Mobile
No:00962788269821 (Jordan)
>00962775401951





--
>To post to this group, send email to
materials-welding@googlegroups.com
>To
unsubscribe from this group, send email to
materials-welding+unsubscribe@googlegroups.com
>For more options, visit this
group's bolg at http://materials-welding.blogspot.com/
>The
views expressed/exchnaged in this group are members personel views
and meant
for educational purposes only, Users must take their own decisions
w.r.t.
applicable code/standard/contract
documents.
--
>To post to this group, send email to
materials-welding@googlegroups.com
>To unsubscribe from this group, send email
to materials-welding+unsubscribe@googlegroups.com
>For more options, visit
this group's bolg at http://materials-welding.blogspot.com/
>The
views expressed/exchnaged in this group are members personel views and
meant for
educational purposes only, Users must take their own decisions w.r.t.
applicable
code/standard/contract documents.
>
--
>To post to this group, send email to
materials-welding@googlegroups.com
>To unsubscribe from this group, send email
to materials-welding+unsubscribe@googlegroups.com
>For more options, visit
this group's bolg at http://materials-welding.blogspot.com/
>The
views expressed/exchnaged in this group are members personel views and
meant for
educational purposes only, Users must take their own decisions w.r.t.
applicable
code/standard/contract documents.
>



--
>
To post to this group, send email to materials-welding@googlegroups.com
>
To unsubscribe from this group, send email to materials-
welding+unsubscribe@googlegroups.com
>
For more options, visit this group's bolg at http://materials-
welding.blogspot.com/
>
The views expressed/exchnaged in this group are members personel views
and meant for educational purposes only, Users must take their own
decisions w.r.t. applicable code/standard/contract documents.
>


Dear Sir,





Thanking You,

Honesty is the best Policy

With Warm Regards,

Muthu Barathi P
Mobile No:00962788269821 (Jordan)
00962775401951

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...