Re: [MW:9613] Expiry period for SMAW consumable-reg

Hi,

There is no code specify the shelf life of electrode, its depends on
the manufacturer recommendation.

I had also faced the problem with Lincoln electrodes certificates, as
they mention in the lot certificates in 1 year. So raised the quarry
in Lincoln Company about the shelf life of electrode; accordingly they
send the warranty/validity certificate (Here I attached the attached
warranty/validity certificates & lot certificates -for your
information)

So when ever you face the shelf life problem with electrode kindly
contact the manufacturer and get the validity confirmation from the
company. its the only record or proof of electrode shelf life and
solution.


Rgs,
Sambath Kumar


On 1/31/11, Ilangkumaran Kumarasamy <ilangkumaran.kumarasamy@borouge.com> wrote:
> Dear Mr Pradip,
>
> Yes your statement is perfectly correct.
>
> Thank you,
> Ilangkumaran
>
> From: materials-welding@googlegroups.com
> [mailto:materials-welding@googlegroups.com] On Behalf Of PREM SHANKARDUTT
> NAUTIYAL
> Sent: Monday, January 31, 2011 1:48 PM
> To: materials-welding@googlegroups.com
> Subject: Re: [MW:9589] Expiry period for SMAW consumable-reg
>
> Hi
>
> Pl. browse the reply already given in earlier thread - MW:4205 :
>
> It's true that boiler or pressure vessel codes or structural welding codes
> do not specify the shelf-life or expiry dates of welding electrodes.
> For example, ASME Nuclear Codes Sec-III, Clause & NB, NC-2440 specifies
> that:- Suitable storage and handling of electrodes, flux, and other welding
> materials shall be maintained. Precautions shall be taken to minimize
> absorption of moisture by fluxes and cored, fabricated, and coated
> electrodes.
>
> The shelf-life of welding electrodes to a great extent depends on electrode
> manufacturer's methods, quality control procedure and how electrodes are
> handled. Depending on the coating type, packing (hermetically sealed or
> not), storing methods and ambient conditions, humidity etc, electrodes may
> last long or less. However as a good practice and based on electrode
> manufacturer's guidelines it may be worth considering:-
>
> * Solid Wires, GTAW/GMAW-No shelf Life.
>
> * Cored Wire -FCAW- No shelf life
>
> * SMAW - The rule should be FIFO (First in First Out). Electrodes where the
> coating shows sign of flaking, cracks etc certainly should be discarded
> without much thoughts. Electrodes not older than 2-3 years but in good
> condition may be used. If required the diffusible hydrogen test could be
> repeated. Electrodes older than 3 years generally should not be used as a
> good engineering rule.
>
> * SAW Fluxes- Shelf life 2-3 years maximum subject to the flux condition and
> amount of fine particles/dust generated and behavior during welding.
> Thanks.
> Pradip Goswami, P.Eng
>
>
>
> Regards
>
> Prem Nautiyal
>
>
>
>
>
> On Mon, 31 Jan 2011 09:48:41 +0530 wrote
>>Dear Experts,
>
> generally what is expiry period for SMAw consumables (Flux coated) dose ASME
> Sec II-C refers regarding this, if so please refer which class.in the
> consumable wraper only manufactured date is given but not the expiry date.
>
>
>
> Thanks & Regards,
>
>
>
> K.Pandiarajan.
>
>
>
>
>
> --
>
> To post to this group, send email to materials-welding@googlegroups.com
>
> To unsubscribe from this group, send email to
> materials-welding+unsubscribe@googlegroups.com
>
> For more options, visit this group's bolg at
> http://materials-welding.blogspot.com/
>
> The views expressed/exchnaged in this group are members personel views and
> meant for educational purposes only, Users must take their own decisions
> w.r.t. applicable code/standard/contract documents.
>
>
>
> PREM S NAUTIYAL
> CELL : 9769316004
> [http://sigads.rediff.com/RealMedia/ads/adstream_nx.ads/www.rediffmail.com/signatureline.htm@Middle]<http://sigads.rediff.com/RealMedia/ads/click_nx.ads/www.rediffmail.com/signatureline.htm@Middle?>
>
> --
> To post to this group, send email to materials-welding@googlegroups.com
> To unsubscribe from this group, send email to
> materials-welding+unsubscribe@googlegroups.com
> For more options, visit this group's bolg at
> http://materials-welding.blogspot.com/
> The views expressed/exchnaged in this group are members personel views and
> meant for educational purposes only, Users must take their own decisions
> w.r.t. applicable code/standard/contract documents.
>
> **********************************************************************
> Borouge is a leading provider of value creating, innovative plastics
> solutions for customers in the Middle East, Asia-Pacific and Africa. Borouge
> employs unique Borstar® technology to produce differentiated products for
> high-value infrastructure applications, including water, gas and industrial
> pipe systems, power and communication cables, advanced packaging and
> automotive components. Borouge's state-of-the-art petrochemical complex is
> located at Ruwais, Abu Dhabi in the United Arab Emirates.
> ===================================================================================
> CONFIDENTIALITY NOTICE
> This email and any files transmitted with it are confidential and intended
> solely for the use of the individual or entity to whom they are addressed.
> If you have received this email in error please delete the email and any
> attachment(s) and notify the sender.
> This footnote also confirms that this email message has been scanned for the
> presence of computer viruses.
> =============================================================================================================
>
>
> --
> To post to this group, send email to materials-welding@googlegroups.com
> To unsubscribe from this group, send email to
> materials-welding+unsubscribe@googlegroups.com
> For more options, visit this group's bolg at
> http://materials-welding.blogspot.com/
> The views expressed/exchnaged in this group are members personel views and
> meant for educational purposes only, Users must take their own decisions
> w.r.t. applicable code/standard/contract documents.
>

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...