Re: [MW:9510] Purging Gas for Fillet Weld

Dear ,
 
You need to provide purging if thk. of SS pipe is less than 6 mm thk. Heat input during fillet welding of support to SS pipe thk.< 6 mm, produces heat tints on ID of pipe,which leads to service failures deoending upon corrosivity of carrying fluid.
 
You can think. of reducing cost of purging by different means
. Above 6 mm SS pipe thk. it is not required.API 582 has got guidence notes.Pl refer.
 
Regards,
 
Manish Kulkarni
--- On Thu, 27/1/11, Suresh <bobsuresh24@gmail.com> wrote:

From: Suresh <bobsuresh24@gmail.com>
Subject: Re: [MW:9505] Purging Gas for F
To: materials-welding@googlegroups.com
Date: Thursday, 27 January, 2011, 9:22 AM

Hi
 
I think NOT required for Fillet welds especially pipe to supports .
 
Suresh

On Thu, Jan 27, 2011 at 8:07 AM, Karthik <karthik6684@yahoo.com> wrote:
No need if it is a support welded on the pipe.But if u welded like end plate (groove+fillet) need.

Thanks & Regards,

(Karthik)

Karthikeyan.S
QA/QC Manager
Getabec Energy Co.,Ltd.
379,Moo6,Soi8,Nikhomphatana,
Rayong-21180,
Thailand.
Phone: 0066 38 897035-8 (Off)
Fax: 0066 38 897034
Hand Phone: 0066 892512282


--- On Wed, 1/26/11, yoga nandhan <yoganandhan@gmail.com> wrote:

From: yoga nandhan <yoganandhan@gmail.com>
Subject: [MW:9489] Purging Gas for Fillet Weld
To: materials-welding@googlegroups.com
Date: Wednesday, January 26, 2011, 6:16 PM



Can anyone please clarify,  for Fillet weld to be carried out in a S.S Pipe (4.5mm wall thickness) to support joint with GTAW Process. Is it required to give Purging Gas in pipe.  (as per Clause 7.5 of API582. (attached)).
 
Pipe Material: SA312 TP316/316L
Support Material: SA240TP316/316L
 
Thickness: 4.5 mm Max.
 
Thanks in advance.

Best Regards,
Yoganandhan Palaniappan
 
--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.



--
Thanks  & Best Regards,

Suresh

Mobile No: 91-92 92 905 905

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...