RE: [MW:27138] IAWS D 1.1 ALLOWS ASME SEC IX WPS/WQT?

When "the Engineer" for the project, as defined in AWS D1.1, approves – the answer is yes.  See the two clauses below:

 

AWS D1.1 Clause "4, §4.2.1.2  - WPS Qualification to Other Standards.  The acceptability of qualification to other standards is the Engineer's responsibility, to be exercised based upon the specific structure, or service conditions, or both.  AWS B2.1-X-XXX Series on Standard Welding Procedure Specifications may, in this manner be accepted for use in this code."

 

AWS D1.1 Clause "4, §4.2.2.1  - Previous Performance Qualification.  Previous performance qualification tests of welders, welding operators, and tack welders that are properly documented are acceptable with the approval of the Engineer.  The acceptability of performance qualification to other standards is the Engineer's responsibility, to be exercised based upon the specific structure, or service conditions, or both.

 

Enjoy

 

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of vicky bhupathi
Sent: Thursday, December 07, 2017 3:18 AM
To: materials-welding@googlegroups.com
Subject: Re: [MW:27136] IAWS D 1.1 ALLOWS ASME SEC IX WPS/WQT?

 

we cannot use ASME IX instead of AWS D1.1 because all the variables were different, in conjunction with both the codes. T,Y,K joints are all added  in structural.  However  depending on the joint configuration we can get approval from the engineer in charge  prior to the production/fabrication.

 

On Dec 7, 2017 12:01 PM, "Hasin Shaikh" <hasin.shaikh@gmail.com> wrote:


Hello To everyone

 

My question about AWS D 1.1 & ASME SEC IX

 

IF i have wps/pqr and welder qualification according to ASME SEC IX can i use the same with structural fabrication and welding with reference of code of AWS D 1.1?

 

or i need to establishe separate WPS/PQR and welder qualification according to AWS D 1.1? 

--

*With Regards
Shaikh.Hasin
Email: hasin.shaikh@gmail.com
Mobile: +91-9924562942*

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...

[MW:5202] RE: 5200] NDT after PWHT

------------------------------------- Interpretation:  I‑89‑14 Subject:         Section I (1986 Edition, 1987 Addenda), PW‑11,                  NDE Prior to PWHT Date Issued:     December 15, 1988 File:            BC88‑393   Question: Does PW‑11 require that NDE be performed on welds after they have been subjected to the postweld heat treatment required by PW‑39?   Reply: No, unless the conditions described in PW‑11.2.2 exist. ---------------------------------------------- Interpretation:  VIII-1-98-09 Subject:         Section VIII, Division 1 (1995 Edition, 1996 Addenda); NDE                 ...