Skip to main content

Re: [MW:27131] Qualifications of welders

Hai all,

What is your final conclusions.
 
Regards, M.S.Viswanathan


On Tuesday, December 5, 2017 9:45 PM, John Henning <jhenning@deltak.com> wrote:


Some care here needs to be applied and please remember to note that this applies only to welder performance qualification.
 
QW-423.1 refers to unassigned base metals.  In the case of unassigned base metals, generally the welder is only qualified for welding the unassigned base metal.
 
However,
 
QW-423.2 allows for base materials produced to other standards that meet the chemical and physical requirements of a P-Number material, to be used as if it were the P-number material for performance qualification.  This is an exception to the general rule stated in QW-423.1 for "unassigned" base metal. 
 
Enjoy
 
John
 
From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of Hasin Shaikh
Sent: Monday, December 04, 2017 11:11 PM
To: materials-welding@googlegroups.com
Subject: Re: [MW:27115] Qualifications of welders
 
Dear  Jhon Sir
 
As per QW 423.1 -unassigned material with similar chemical composition also included, 
in that case no need to go further new performance qualification if unassigned material have similar chemical composition with previous any qualification ,
 
This is my interpretation, is correct or not please advise.
 
With Regards
Hasin Shaikh
 
On Mon, Dec 4, 2017 at 9:22 PM, John Henning <jhenning@deltak.com> wrote:
No welder requalification is not required, provided all other requirements of QW-353 are met, and only Section IX qualification is required..
 
While Table QW-353 states QW-403.18 is an essential variable one has to look further.  QW-403.18 states:
 
 
So one has to look again further at QW-423, Alternate Base Materials for Welder Qualification:  There is no distinction made between P8 and P10H as far base material required is concerned.  In fact the welder could have qualified using P1  base materials for both P8 and P10H base metals.
 
However, customer requirements may restrict qualification. 
 
Clearly, applying the first instance in QW-423.1, performance qualification with P8 material
 
From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of PGoswami
Sent: Monday, December 04, 2017 9:28 AM
To: materials-welding@googlegroups.com
Subject: RE: [MW:27111] Qualifications of welders
 
 
A new qualification is required in this case. Qualification on other austenitic stainless steels(P No 8) does not permit the validity of qualification for duplex stainless steels (P No 10H). It's clearly stated under QW-353, please see the extract below.
 
F No for both ASS and DSS are the same, F5 for SMAW (SFA 5.5) and F6 for GTAW/GMAW(SFA 5.9).
 
Thanks.
 
 
 
P.Goswami.P.Eng, IWE.
Welding & Metallurgical Specialist
 
 
QW-351 GENERAL
A welder shall be requalified whenever a change is
made in one or more of the essential variables listed for
each welding process
 
 
 
 
From: 'ms viswanathan' via Materials & Welding [mailto:materials-welding@googlegroups.com]
Sent: December 4, 2017 7:23 AM
To: materials-welding@googlegroups.com
Subject: Re: [MW:27109] Qualifications of welders
 
Yes, I agree .Thanks for your guidance.
 
Regards, M.S.Viswanathan
 
On Monday, December 4, 2017 1:46 PM, Kannayeram Gnanapandithan <kgpandithan@gmail.com> wrote:
 
MSV
            pl see QW 416,423.
 A no is at all essential variable for welding performance qualification. Let us not misguide the people. 
 
Virus-free. www.avast.com

THANKS & BEST REGARDS,
KG.PANDITHAN, BE, IWE,  AWS-CWI, CSWIP 3.1,
CONSULTANT-WELDING & QUALITY
Mobile no: +919940739349
 
On Mon, Dec 4, 2017 at 3:51 PM, 'ms viswanathan' via Materials & Welding <materials-welding@googlegroups.com> wrote:
No, because DSS - P number is 10H and A.No-7 and .S.S-   P number is -8 and A.No 8 , essential variables.
 
Regards, M.S.Viswanathan
 
On Monday, December 4, 2017 12:42 PM, foued oudina <oudinafou21@gmail.com> wrote:
 
Dear Colleagues ;
 
 
Could you  please help me, we have welders qualified in SS they can weld DSS.
 
Thanks
 
 
 
 
 
OUDINA FOUAD | QC Welding OFF PLOT
 
Técnicas Reunidas Group
TouatGaz Project – EPCC Processing & Production Facilities
Field Engineering Group                   
Oued Zine, Adrar, Algeria
( Ext. 3912
 
 
--
https://materials-welding. blogspot.com/
https://www.linkedin.com/ groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to
materials-welding+unsubscribe@ googlegroups.com.
Visit this group at
https://groups.google.com/ group/materials-welding.
For more options, visit
https://groups.google.com/d/ optout.
 
--
https://materials-welding. blogspot.com/
https://www.linkedin.com/ groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@ googlegroups.com.
Visit this group at https://groups.google.com/ group/materials-welding.
For more options, visit https://groups.google.com/d/ optout.
 
--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.
 
--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.
--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.
--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.


 
--
*With Regards
Shaikh.Hasin
Email: hasin.shaikh@gmail.com
Mobile: +91-9924562942*

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.
--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.


Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...

[MW:5202] RE: 5200] NDT after PWHT

------------------------------------- Interpretation:  I‑89‑14 Subject:         Section I (1986 Edition, 1987 Addenda), PW‑11,                  NDE Prior to PWHT Date Issued:     December 15, 1988 File:            BC88‑393   Question: Does PW‑11 require that NDE be performed on welds after they have been subjected to the postweld heat treatment required by PW‑39?   Reply: No, unless the conditions described in PW‑11.2.2 exist. ---------------------------------------------- Interpretation:  VIII-1-98-09 Subject:         Section VIII, Division 1 (1995 Edition, 1996 Addenda); NDE                 ...