Re: [MW:7957] NAXTRA M700 weldebility

For this materilal you can use either E11016 or E11018M elctrode (Atom arc / Hobart Hobaaloy brand has electodres readily avaible) For SAW wire ECM2 & FCAW E111T1K3MJ can be used (Lincon brand) . Generally this materials are used for low temp application (-40°C)
Preheat & Post heat is mandetory for this material

On Sun, Oct 31, 2010 at 7:46 AM, Prakash Hegde <pb.hegde@yahoo.com> wrote:
 
 
 
Netra material being high  strength material which we have tried with E11016 type elctrode and SAW wire which require to achieve impact at minus 40C and higher UTSatroom room temp (This  material is similar to SA517 gr F or similar)
Welding of this material is critical from resulted properties point of view W
Welding parameters are to be estblished with batch testing in 3G position for electrodes with controlled bead length , current, volt to estblish heat input. and  also preheating and post heating temp.Some time you may require to have ISR for restrain joint
 
generaly Kobelco or Thyssen make brand are good which we have used
 
Regards
 
Hegde P.B.
 
 

 


From: Dick Overkleeft <dick.overkleeft@gmail.com>
To: materials-welding@googlegroups.com
Sent: Sat, 30 October, 2010 11:21:47 PM
Subject: [MW:7950] NAXTRA M700 weldebility

We are going to use above material fro shipbuilding purpose. Thickness 30- 40 mm. We do not have experience with this specified material, I would like to know from your experience information on ;
Ceq and impactvalue in L and T direction.
 
In regard to the attached manufacturers information , the deviation in chemical composition may be rather high.
 
This may require preheating, which influences the weldebility. If you have any practical information, it will be appreciated.
 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...