Skip to main content

FW: Fw: [MW:7844] ASME BPV SEC IX Material Range issue

 

 

From: John Henning
Sent: Tuesday, October 26, 2010 3:20 PM
To: John Henning
Subject: RE: Fw: [MW:7798] ASME BPV SEC IX Material Range issue

 

Further it appears that Karthik made a typing error – there is no P-Number 2 – I believe where he wrote P-Number 2 Group-Number 2 he meant to type P-Number 1 Group Number 2.  This is the only thing that makes any sense.

 

John

 

From: John Henning
Sent: Tuesday, October 26, 2010 3:13 PM
To: 'materials-welding@googlegroups.com'
Subject: RE: Fw: [MW:7798] ASME BPV SEC IX Material Range issue

 

K. Babu

 

You are incorrect.

 

QW-403.5 addresses Group number restrictions for base metals when impact testing is required.

 

Please review QW-403.5, end of third paragraph:  "For ferrous materials . . . In addition, when base metals of two different P-Number  Group Number combinations are qualified using a single test coupon, that coupon qualifies the welding of those two P-Number Group Numbers to themselves as well as to each other using the variables qualified."

 

 

Please also note the following Code update notification (from HSB web site):

Addenda:

A06

Code Book:

IX

Subpart or Table:

Article IV

Code Paragraph:

QW-403.5

ASME Tracking Number:

BC03-1063

Part:

 

Subject:
Clarify Qualification Requirements for Dissimilar Welds

Description:
Revised QW-403.5 to clarify that different PQRs qualified for base metals within the same P-No., but having different Group numbers, may be used to support welding the different group numbers to each other in combination, provided all remaining essential and supplementary essential variables are the same.

 

So as  of the 2006 Addenda of Section IX – the proposal to write three WPS's {P1G1 –P1G1, P1G2-P1G2, and P1G1-P1G2} is valid and correct.

 

Obviously if impacts are not required, Group Number is superfluous, and all P1materials are qualified to weld to all P1 materials.

 

John.

 

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of Kathalingam Babu
Sent: Monday, October 25, 2010 7:56 PM
To: materials-welding@googlegroups.com
Subject: Re: Fw: [MW:7798] ASME BPV SEC IX Material Range issue

 

Aneesh,

 

Regarding the Query No.2, the actual PQR is P1 G1  to P1  G2. So is it possible to weld P2 G2 to P2 G2 as per QW 403.5?

 

You cannot weld P2 G2 to P2 G2  with existing P1 G1  to P1  G2 qualification

 

Regards

 

K.Babu

 

 

----- Original Message -----

From: Karthik

Sent: Monday, October 25, 2010 11:31 PM

Subject: Re: Fw: [MW:7793] ASME BPV SEC IX Material Range issue

 

Hi,

Yes. Can write if impact test is not applicable.

 

Thanks & Regards

 

(Karthik)



 

Karthikeyan.S

QA/QC Manager

Getabec Energy Co.,Ltd.

379,Moo6,Soi8,Nikhomphatana,

Rayong-21180,

Thailand.

Phone: 0066 38 897035-8 (Off)

Fax: 0066 38 897034

Hand Phone: 0066 892512282



--- On Mon, 10/25/10, aneesh <aneeshgopi22@rediffmail.com> wrote:


From: aneesh <aneeshgopi22@rediffmail.com>
Subject: Fw: [MW:0] ASME BPV SEC IX Material Range issue
To: "Materials & Welding" <materials-welding@googlegroups.com>
Date: Monday, October 25, 2010, 8:28 PM

Karthik Sir,

Regarding the Query No.2, the actual PQR is P1 G1  to P1  G2. So is it possible to weld P2 G2 to P2 G2 as per QW 403.5?

Please correct me if I am wrong.

Regards,
Aneesh
KSA




On Mon, 25 Oct 2010 11:32:50 , Karthik wrote

Hi,

.As per QW403.5 you can use.Please find below the answer for your quiries marked in RED.

Quiery No.1

1. Is there any problem for welding P1 Group No.1 to P1 Group No.1  &  P1 Group No.2 to P1 Group No.2 based on above PQR?

QW403.5

For ferrous materials in table QW/QB-422, a procedure

qualification shall be made for each P-Number Group Number

combination of base metals, even though procedure

qualification tests have been made for each of the two

base metals welded to itself. If, however, two or more

qualification records have the same essential and supplementary

essential variables, except that the base metals

are assigned to different Group Numbers within the same

P-Number, then the combination of base metals is also

qualified. In addition, when base metals of two different

P-Number Group Number combinations are qualified using

a single test coupon, that coupon qualifies the welding of

those two P-Number Group Numbers to themselves as well

as to each other using the variables qualified.

This variable does not apply when impact testing of the

heat-affected zone is not required by other Sections.

Quiery No.2

2.  Can I write separate WPS (with impact test) based on above PQR for,

Material – P1 Group No. 1 to P1 Group No. 1

Material – P2 Group No. 2 to P2 Group No. 2

QW200.2 (f) Multiple WPSs With One PQR/Multiple PQRs With

One WPS. Several WPSs may be prepared from the data

on a single PQR (e.g., a 1G plate PQR may support WPSs

for the F, V, H, and O positions on plate or pipe within

all other essential variables). A single WPS may cover

several essential variable changes as long as a supporting

PQR exists for each essential and, when required, supplementary

essential variable [e.g., a single WPS may cover

a thickness range from 1⁄16 in. (1.5 mm) through 11⁄4 in.

(32 mm) if PQRs exist for both the 1⁄16 in. (1.5 mm) through

14

3⁄16 in. (5 mm) and 3⁄16 in. (5 mm) through 11⁄4 in. (32 mm)

thickness ranges].

 

Quiery No.3

Is there any problem for showing all material range in a single WPS based on above PQR?

Ie, qualified range of materials- P1 Group No. 1 & P1 Group No. 2 in the same WPS.

No problem.You can write all material range as much as possible within the P number specified in the WPS

Thanks & Regards,

 

(Karthik)

Karthikeyan.S

QA/QC Manager

Getabec Energy Co.,Ltd.

379,Moo6,Soi8,Nikhomphatana,

Rayong-21180,

Thailand.

Phone: 0066 38 897035-8 (Off)

Fax: 0066 38 897034

Hand Phone: 0066 892512282



--- On Sun, 10/24/10, limesh M <limesh78@gmail.com> wrote:


From: limesh M <limesh78@gmail.com>
Subject: [MW:7767] ASME BPV SEC IX Material Range issue
To: "Materials & Welding" <materials-welding@googlegroups.com>
Date: Sunday, October 24, 2010, 9:42 PM

Dear All,

 

I need your help in the following subject.

 

Design Code – ASME B31.3

Welding Code – ASME BPV SECTION IX

I have a PQR for the following material classification as per ASME BPV SEC IX

Material – P1 Group No. 1 to P1 Group No. 2

Weld Metal Impact Tested – Yes

My query is that,

1. Is there any problem for welding P1 Group No.1 to P1 Group No.1  &  P1 Group No.2 to P1 Group No.2 based on above PQR?

2.  Can I write separate WPS (with impact test) based on above PQR for,

Material – P1 Group No. 1 to P1 Group No. 1

Material – P2 Group No. 2 to P2 Group No. 2

My next query is that,

Is there any problem for showing all material range in a single WPS based on above PQR?

Ie, qualified range of materials- P1 Group No. 1 & P1 Group No. 2 in the same WPS.

 

 

Regards,

 

Limesh

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...