Re: [MW:7872] WQT-Visual Acceptance Criteria Issue

Dear Limesh,

If u r doing by ASME B31.3, then u have to refer B31.3 acceptance criteria. Chapter 6.

Thanks & Regards
M

On Wed, Oct 27, 2010 at 11:23 AM, Karthik <karthik6684@yahoo.com> wrote:
Hi,
You are correct.But Sec.IX acceptance criteria is a minimum requirement.However as per QW301.2 specifies that if manufacturer or his superviso feels that the welder/operator can not produce satisfactory results (apart from sec.IX...i.e undercut,porosity etc.,) he may reject his qualification.Pls.find below the extraction.
 

QW301.2 (last pragraph)

The performance test may be terminated at any stage of

the testing procedure, whenever it becomes apparent to the

supervisor conducting the tests that the welder or welding

operator does not have the required skill to produce satisfactory

results.

So it is a manufacturer's responsibilty to qualify a welder/operator's qualifications to meet the code specification and acceptance criteria as well as to the company's quality system.
 
I hope it is clear to you.
 
Thanks & regards,
 
(Karthik)
Karthikeyan.S
QA/QC Manager
Getabec Energy Co.,Ltd.
379,Moo6,Soi8,Nikhomphatana,
Rayong-21180,
Thailand.
Phone: 0066 38 897035-8 (Off)
Fax: 0066 38 897034
Hand Phone: 0066 892512282


--- On Wed, 10/27/10, limesh M <limesh78@gmail.com> wrote:

From: limesh M <limesh78@gmail.com>
Subject: Re: [MW:7858] WQT-Visual Acceptance Criteria Issue
To: materials-welding@googlegroups.com
Date: Wednesday, October 27, 2010, 12:40 PM


Dear Raghuram Sir & Karthik sir,
 
Thank you very much for the prompt reply.Based on this only I can ask remaining thing in my mind.
 
 
Dear All,
 
I reviewed following clauses of ASME BPV SEC IX.
 

QW-142 Special Examinations for Welders

Radiographic or ultrasonic examination per QW-191may be substituted for mechanical testing of QW-141 for

groove-weld performance qualification as permitted in QW-304 to prove the ability of welders to make sound

welds.

 

QW-143 Examination for Welding Operators

Radiographic or ultrasonic examination per QW-191 may be substituted for mechanical testing of QW-141 for groove weld performance qualification as permitted in QW-305 to prove the ability of welding operators to make sound welds.

 

QW-144 Visual Examination

Visual examination as described in QW-194 is used to determine that the final weld surfaces meet specified quality

standards.

QW-194 Visual Examination — Performance

Performance test coupons shall show complete joint penetration with complete fusion of weld metal and base metal.

 

QW-302.2 Volumetric NDE.

 

When the welder or welding operator is qualified by volumetric NDE, as permitted in QW-304 for welders and QW-305 for welding (10) operators, the minimum length of coupon(s) to be examined shall be 6 in. (150 mm) and shall include the entire weld circumference for pipe(s), except that for small diameter pipe, multiple coupons may be required, but the number need not exceed four consecutively made test coupons. The examination technique and acceptance criteria shall be in accordance with QW-191.

 

QW-191 Volumetric NDE

QW-191.1 Radiographic Examination

QW-191.1.1 Method.

The radiographic examination in QW-142 for welders and in QW-143 for welding operators shall meet the requirements of Article 2, Section V,except as follows:

(a) a written radiographic examination procedure is not required. Demonstration of density and image quality

requirements on production or technique radiographs shall be considered satisfactory evidence of compliance with

Article 2 of Section V

(b) final acceptance of radiographs shall be based on the ability to see the prescribed image and the specified

hole of a hole-type image quality indicator (IQI) or the designated wire of a wire-type IQI. The acceptance standards

of QW-191.1.2 shall be met.

 

 

QW-191.1.2.3 Production Welds. The acceptance criteria for welders or welding operators who qualify on

production welds by radiography as permitted in QW-304.1 or QW-305.1 shall be per QW-191.1.2.2.

 

 

 

 

My query is that, QW 194 is dealing with complete joint penetration and fusion only. What is the acceptance criteria for cap and root under cut,arc strikes,bead profile?Why ASME  BPV is silent on remaining defects ? 

 

 

Regards,

 

 

Limesh

 

 

On Wed, Oct 27, 2010 at 8:44 AM, Bathula Raghuram (Mumbai - PIPING) <R.Bathula@ticb.com> wrote:

QW302.4, QW194

"Performance test coupons shall show complete joint penetration with complete fusion of weld metal and base metal".

 

 

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of limesh M
Sent: Wednesday, October 27, 2010 10:03 AM
To: Materials & Welding
Subject: [MW:7847] WQT-Visual Acceptance Criteria Issue

 

Dear All,

 

Design Code - ASME B31.3

Welding Code - ASME BPV SEC IX

 

I want to qualify some welders and welding operators based on ASME BPV SEC IX.

What is the visual acceptance criteria as per code (Suppose there is no client specification regarding this matter)?

Please mention the relevant code clauses for reference.

 

 

Regards,

 

 

Limesh


--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...