Re: [MW:18528] Ferrite Content Check on root or final weld

  
You can use AWS/SFA E 316L-15 ( IS E19.12.2.LB20), an extra low carbon 17/14/2.5 Mo type SS basic coated
electrode with good corrosion resistance qualities.
This electrode is exceptionally good for welding AISI 316,316L, 317L & 318 type  material and provides a maximum
of 2.0 % ferrite . Such electrodes are designed for urea reactors and similar chemical equipment  used for temperature
services.
Typical chemistry:
C - 0.03 max.,         Mn 1.0 to 2.50,        Si- 0.20 to 0.45,          Cr – 17.0 to 18.50,         Ni – 13.0 to 14.0,     
Mo- 2.0 to 3.0,         S/P 0.02 max.                Ferrite content – 2.00 max.
UTS: 520-630 Mpa.         El % – 35 to 45     &     impact of 60 to 100 joules at 27±20 C.
 
On same basis,  E 316-L – 16 (LF) type special  Electrodes are also available with ferrite less than 0.50%.
C - 0.03 max.,         Mn 5.0 to 7.0,        Si- 0.30 to 0.80,          Cr – 17.0 to 20.00,         Ni – 13.0 to 16.0,     
Mo- 2.0 to 3.0,         S/P 0.02 max.                Ferrite content – 2.00 max.
UTS: 520-630 Mpa. El %– 35 to 45 and impact of 30 to 75 joules at -1960 C.
Corrosion rate as per ASTM  A262 practice C  is 0.50 grams per m2/hr. Max. – 22 mpy.
 
All above electrodes are made to order  and may be available with leading electrode manufactures
like Adore, Esab, D & H, GE  and others  in our country.
Similarly you can scout for equivalent TIG  filler wires also after stipulating  your requirement from
manufactures from abroad or any  of their local agencies in India.
 
Sridhar.
--------------------------------------------------------------------------------------------------------------------------------------------------------------- 
 
From: HAREESH K V <hareesh13h@gmail.com>
To: materials-welding <materials-welding@googlegroups.com>
Sent: Tuesday, 27 August 2013 10:05 AM
Subject: Re: [MW:18523] Ferrite Content Check on root or final weld
As per my opinion,

1. check the ferrite number of the base metal. 
2.Select a consumable batch having a ferrite number such that the average ferrite number of the base metal and the consumable is with in the range what required for you. Normally after welding an average ferrite number will be in the weld.
3. Do a sample weld and check the ferrite number. 
4. For the same manufacturer and brand name there will be slight variations in the ferrite number. So check the batch certificate and select a batch having a low ferrite number. Also do a small weld pad and check whether the ferrite number you are getting (Using your ferrite meter) is same as in batch certificate.
5. Also
keep the heat input to the minimum possible and keep the cooling rate to the minimum possible.
On Sun, Aug 25, 2013 at 8:10 PM, Prakash Hegde <pb.hegde@yahoo.com> wrote:
Dear Mr Ankit
i) The weld ment Ferrite to be checked after final Weld However the depth at which the ferrite to be checked depends upon spec requirement
ii) For  to get Ferrite between 2-5 is very low hence generaly Nil Ferrite consumables are to be used (also Basic coated electrodes are being used) where you require to take extra precaution during welding to avoid Hot Crack(Shrinkage Crack)
 
Regards
Hegde P.B.

From: Ankit PAtel <ankit.patel@orientalindia.net>ence
To: materials-welding@googlegroups.com
Sent: Saturday, 24 August 2013 6:00 PM
Subject: [MW:18506] Ferrite Content Check on root or final weld
Dear Exerts,
 
Kindly suggest on following issue
We have a job on which ferrite content test is essential. we are welding with root run by GTAW & sub sequent layer by SMAW. Please confirm whether it is essential to check the ferrite content of the root or final weld.(top of the weld.)
Base Material-SA 240 TP 316L
Filler Wire/Electrode:- ER-316L & E-316L
Also our requirement is 2FN to 5FN kindly suggest any filler wire/Electrode manufacturer.
 
Regards
 
Ankit Patel
Engineer Quality
Oriental Manufacturers Private Limited
A: P.C.C. Notified Area, Ranoli Station Road,
 Ranoli -391 350 Baroda Gujarat India
T: +91.265.223 1663/2232936
 
 
-- To post to this group, send email to materials-welding@googlegroups.comTo unsubscribe from this group, send email to mailto:materials-welding%2Bunsubscribe@googlegroups.comFor more options, visit this group's bolg at http://materials-welding.blogspot.com/http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.--- You received this message because you are subscribed to the Google Groups "Materials & Welding" group.To unsubscribe from this group and stop receiving emails from it, send an email to mailto:materials-welding%2Bunsubscribe@googlegroups.com.For more options, visit https://groups.google.com/groups/opt_out.
-- To post to this group, send email to materials-welding@googlegroups.comTo unsubscribe from this group, send email to mailto:materials-welding%2Bunsubscribe@googlegroups.comFor more options, visit this group's bolg at http://materials-welding.blogspot.com/http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.--- You received this message because you are subscribed to the Google Groups "Materials & Welding" group.To unsubscribe from this group and stop receiving emails from it, send an email to mailto:materials-welding%2Bunsubscribe@googlegroups.com.For more options, visit https://groups.google.com/groups/opt_out.
--
----------------------
Hareesh K V
+91-9447625012

-- To post to this group, send email to materials-welding@googlegroups.comTo unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.comFor more options, visit this group's bolg at http://materials-welding.blogspot.com/http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.--- You received this message because you are subscribed to the Google Groups "Materials & Welding" group.To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.For more options, visit https://groups.google.com/groups/opt_out.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...