Skip to main content

Re: [MW:12544] Hydrotest-API 650

On 5/3/11, DHANASEKARAN SUBRAMANIAM <subramaniamdhanasekaran7@gmail.com> wrote:
> Gents,
>
> Pad plate for pipe support has been welded with tank shell before hydrotest.
> After hydrotest we have done fitup of pipe support on the pad plate which
> was already welded with shell.
> To avoid distortion during the welding 2 stiffner support provided both
> sides of the pipe support and welded less than 1'' tack weld with the low
> hydrogen electrode|(E-7018).
>
> Please see the attached figure for your referrence.
>
>
>
> 2011/5/2 Jorge Mejía Lema <jmejialema@gmail.com>
>
>> Please read the following para gphs API 650 , Eleven Edition:*
>>
>> 7.2.1.11
>> *Non-structural small attachments such as insulation clips, studs and pins
>> but not insulation support rings or bars may
>>
>> be welded by the arc stud, capacitor discharge or shielded metal arc
>> process to the exterior of the shell including reinforcing plates
>>
>> or PWHT assemblies and roof either before or after hydrostatic testing is
>> performed, but before the tank will be filled with product
>>
>> provided:
>>
>> a. The attachment locations meet the spacing requirements of 5.8.1.2a.
>>
>> b. The arc stud welding process is limited to 10 mm (
>> 3/8 in.) maximum diameter studs or equivalent cross-section.
>>
>> c. The maximum shielded metal arc electrode is limited to 3 mm (
>> 1/8 in.) diameter and shall be a low-hydrogen type.
>>
>> d. The attachment welds, except for those made by the capacitor discharge
>> method, shall be inspected per 7.2.3.5. The attachment
>>
>> welds made by the capacitor discharge method shall be visually examined
>> for
>> all types and groups of shell materials.
>>
>> e. All stud welding and capacitor discharge procedures have been qualified
>> in accordance with ASME Section IX. Capacitor discharge
>>
>> procedures do not require procedure qualification provided the power
>> output
>> is 125 watt-sec or less.
>>
>> The shielded metal arc weld procedures shall meet the requirements of
>> Section 9 for qualification for use.
>> *
>>
>> 7.3.6 Hydrostatic Testing Requirements
>>
>> 7.3.6.1
>> *This hydrostatic test of the tank shall be conducted before permanent
>> external piping is connected to the tank. Attachments
>>
>> to the shell defined in 5.8.1.1, located at least 1 m (3 ft) above the
>> water level, and roof appurtenances may be welded during the filling
>>
>> of the tank. After completion of the hydro-test, only non-structural small
>> attachments may be welded to the tank in accordance
>>
>> with 7.2.1.11. Any welded joints above the test-water level shall be
>> examined for leakage by one of the following methods:
>> Regards,
>> Jorge Mejía, Colombia, South America
>>
>> 2011/5/1 <rosli@labuanship.com>
>>
>>> Dhana,
>>>
>>> You need to redo the HT if the welding of temporary support attached to
>>> pressure part, refer to your tank construction code. Thanks
>>>
>>> Regards
>>> RM
>>>
>>> Sent by Maxis from my BlackBerry® smartphone
>>> ------------------------------
>>> *From: *SOHAIB GHNAIMAT <sohaib_cegco@yahoo.com>
>>> *Sender: *materials-welding@googlegroups.com
>>> *Date: *Sun, 1 May 2011 10:16:21 -0700 (PDT)
>>> *To: *<materials-welding@googlegroups.com>
>>> *ReplyTo: *materials-welding@googlegroups.com
>>> *Subject: *Re: [MW:10909] Hydrotest-API 650
>>>
>>> Re-Hydro test should be done.
>>>
>>> Regards,
>>>
>>> Sohaib
>>>
>>> ------------------------------
>>> *From:* DHANASEKARAN SUBRAMANIAM <subramaniamdhanasekaran7@gmail.com>
>>> *To:* materials-welding@googlegroups.com
>>> *Sent:* Sun, May 1, 2011 8:40:39 AM
>>> *Subject:* [MW:10902] Hydrotest-API 650
>>>
>>> Gents,
>>> After the completion of a tank hydro test, some temporary attachment
>>> welding has been made on the shell and roof plates.
>>> What action needs to be taken at this stage, kindly provide the action
>>> plan with code references.
>>>
>>>
>>> Your Immediate response is highly appreciated.
>>>
>>>
>>>
>>>
>>> --
>>> *WITH REGARDS*,
>>> *DHANASEKARAN .S ,*
>>> *Mob.no <http://mob.no/>: +96893220429.
>>> *
>>>
>>> --
>>> To post to this group, send email to materials-welding@googlegroups.com
>>> To unsubscribe from this group, send email to
>>> materials-welding+unsubscribe@googlegroups.com
>>> For more options, visit this group's bolg at
>>> http://materials-welding.blogspot.com/
>>> The views expressed/exchnaged in this group are members personel views
>>> and
>>> meant for educational purposes only, Users must take their own decisions
>>> w.r.t. applicable code/standard/contract documents.
>>>
>>> --
>>> To post to this group, send email to materials-welding@googlegroups.com
>>> To unsubscribe from this group, send email to
>>> materials-welding+unsubscribe@googlegroups.com
>>> For more options, visit this group's bolg at
>>> http://materials-welding.blogspot.com/
>>> The views expressed/exchnaged in this group are members personel views
>>> and
>>> meant for educational purposes only, Users must take their own decisions
>>> w.r.t. applicable code/standard/contract documents.
>>>
>>> --
>>> To post to this group, send email to materials-welding@googlegroups.com
>>> To unsubscribe from this group, send email to
>>> materials-welding+unsubscribe@googlegroups.com
>>> For more options, visit this group's bolg at
>>> http://materials-welding.blogspot.com/
>>> The views expressed/exchnaged in this group are members personel views
>>> and
>>> meant for educational purposes only, Users must take their own decisions
>>> w.r.t. applicable code/standard/contract documents.
>>>
>>
>>
>>
>> <http://www.chiefsmilies.com/wp/ie.php?plg=ie&subs=gmail&elm=sign>
>>
>> --
>> To post to this group, send email to materials-welding@googlegroups.com
>> To unsubscribe from this group, send email to
>> materials-welding+unsubscribe@googlegroups.com
>> For more options, visit this group's bolg at
>> http://materials-welding.blogspot.com/
>> The views expressed/exchnaged in this group are members personel views and
>> meant for educational purposes only, Users must take their own decisions
>> w.r.t. applicable code/standard/contract documents.
>>
>
>
>
> --
> *WITH REGARDS*,
> *DHANASEKARAN .S ,*
> *Mob.no: +96893220429.
> *
>
> --
> To post to this group, send email to materials-welding@googlegroups.com
> To unsubscribe from this group, send email to
> materials-welding+unsubscribe@googlegroups.com
> For more options, visit this group's bolg at
> http://materials-welding.blogspot.com/
> The views expressed/exchnaged in this group are members personel views and
> meant for educational purposes only, Users must take their own decisions
> w.r.t. applicable code/standard/contract documents.
>

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...