RE: [MW:12555] defect on circ-seam of H2 service vessel

In my opinion- yes, as per UG 99(a)(1), I consider it as major repair, as you are welding almost 20% of thickness.

 

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of hrishikm07@gmail.com
Sent: Tuesday, September 27, 2011 3:17 PM
To: Materials Welding
Subject: Re: [MW:12554] defect on circ-seam of H2 service vessel

 

The defect is visually confirmed; nothing is assumed. I want to conclude that for repair of this dimension does the code call for rehydro?

Regards
Hrishi

Sent on my BlackBerry® from Vodafone


From: "Bathula Raghuram (Mumbai - PIPING)" <R.Bathula@ticb.com>

Sender: materials-welding@googlegroups.com

Date: Tue, 27 Sep 2011 13:01:44 +0530

To: 'materials-welding@googlegroups.com'<materials-welding@googlegroups.com>

ReplyTo: materials-welding@googlegroups.com

Subject: RE: [MW:12551] defect on circ-seam of H2 service vessel

 

did you compare this image with the RT taken at fab shop? Did you conclude anything why it was happened?

Did you check visually and measured these dimensions or assumption from the RT image?  Images like this are possible May be due to the thickness difference of shell and dished end. If it is visually confirmed, yes repair by welding is required followed by local PWHT/NDT/hardness check and re hydro

 

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of K.M Hrishikesan
Sent: Tuesday, September 27, 2011 11:44 AM
To: materials-welding
Subject: [MW:12548] defect on circ-seam of H2 service vessel

 

Dear Mr. Pradeep Goswami & other experts...

 

We have a newly fabricated Vessel having following details

 

 

Vessel:  1200 mm ID X 4550 mm TL-TL

MOC: SA 516 Gr 60

Code of constr: ASME section VIII div 1 2007 edn.

Thickness: shell-20mm; DE-24 mm

Design pr- 32.3 kg/sq.cm; Design temp - 80 deg.C

Service: LPG+Naphtha ; Vessel is designed for  Hydrogen service, 100%RT, Fully PWHT; hydrotested ,cleared by TPI, erected at site, yet to be commissioned

 

 

Imperfection (a notch or gouge out)of about 3-4 mm deep and 15 mm long observed on weld seam CS-1 (Top Dished end to shell circ. seam joint ) from inside of vessel. Please see the attached image of segment radiographed by us.

 

My queries...

 

What rectification shall I do on the defective segment on the service point of view?

What are the NDE's required?

Is a local PWHT mandatory at the repaired segment?

Any special precautions for H2 service...

 

appreciate your quick feedbacks..

 

Regards

Hrishi

 


Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...