Skip to main content

[MW:12523] RE: 12516] WPS Heat treatment condition

Hi Vijay,
 
As per QW 407.2 a change of PWHT time and temperature is a supplementary essential variable. If there is no requirement of impact properties, the PQR qualified @ 620 deg C of PWHT  may be used as the supporting PQR for performing PWHT @ 670 deg C.
 
Note:- selection of 670 deg C for PWHT would not be right for P1 material due to the fact that it would significantly soften carbon steel.If there is any hardness restriction then the PQR  and the production weld should be done at the same Time and Temperature.
 
Austenitic stainless steels do not require any PWHT ( in the temperature region of 600-700 deg C),except for solution annealing(1000-1040 deg C) to improve mechanical properties and corrosion resistance.
 
Thanks.
 
 
Pradip Goswami,P.Eng.IWE
Welding & Metallurgical Specialist & Consultant
Ontario,Canada.
Email-pgoswami@sympatico.ca,
 


From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of Vijay Katkar
Sent: Saturday, September 24, 2011 11:06 AM
To: materials-welding@googlegroups.com
Subject: [MW:12516] WPS Heat treatment condition

Dear All,

Regarding heat treatment ,

I have P1 to P8 PQR with following heat treatment,

 

Loading temperature :- 350  ̊C 

 heating rate : 70   ̊C  /hr

Soaking temperature: 620  ̊C

Cooling rate : 70  ̊C/hr

Unloading temperature: 350  ̊C

 

our job requirement is

Loading temperature :- 350  ̊C

heating rate : 70  ̊C/hr

Soaking temperature: 670  ̊C

Cooling rate : 70  ̊C/hr

Unloading temperature: 350  ̊C

 

Is it possible to use above PQR for same job if yes please tell me the reference in section IX. or this not possible then why because above all temperature below lower critical temperature..

please advice your valuable experience..............

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...