RE: [MW:11492] VACUUM TEST FOR SOTRAGE TANKS ROOF AS PER API 650

Dear John,

 

If the roof is not having atmospheric vent, you have to test roof in following way mentioned in API 650 2010 7.3.7.1

 

7.3.7 Testing of the Roof

7.3.7.1 Upon completion, the roof of a tank designed to be gas-tight (except for roofs designed under 7.3.7.2, F.4.4, and F.7.6)

shall be tested by one of the following methods:

a. Applying internal air pressure not exceeding the weight of the roof plates and applying to the weld joints a bubble solution or

other material suitable for the detection of leaks.

b. Vacuum testing the weld joints in accordance with 8.6 to detect any leaks.

7.3.7.2 Upon completion, the roof of a tank not designed to be gas-tight, such as a tank with peripheral circulation vents or a

tank with free or open vents, shall receive only visual inspection of its weld joints, unless otherwise specified by the Purchaser.

 

For B, its simple to do Vacum box test

For A, you can make the internal pressure ( By U tube manometer, may be it will be 50 or 60 mm of water column) during the hydrotest.

 

With regards,

S. Sivasubramanian.

 

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of Rajagopal Kannan
Sent: Monday, June 27, 2011 1:31 PM
To: materials-welding@googlegroups.com
Subject: Re: [MW:11488] VACUUM TEST FOR SOTRAGE TANKS ROOF AS PER API 650

 

Dear John,

No, Roof do not require vacuum testing. If you have access to both the sides of roof, you can deploy and NDT for weld examination.

Thanks and best Regards,

K.Rajagopal

On Sun, Jun 26, 2011 at 10:25 AM, manoj john <manojacgnr@gmail.com> wrote:

Dear All experts,

Please give me information about vacuum test of roof for storage tanks
as per API 650.

I am fabricating sotrage tanks as per API 650 with fixed roof with
open vent nozzle and designed for Atmospheric pressure.

My doubt is whether this tank roof require vacuum testing as per API 650.


Thanks and Best Regards.

John Abraham

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...