Skip to main content

Re: [MW:22544] Re: Titanium tube welding and cooling time required

Dear Sekhar

What is important for Ti welding is the Cleanliness.  A dust free atmosphere, clean surface and consumables and the right parameters shall produce a good quality welding. A change of 5deg C temperature due to AC is not going to make any difference to weld quality but may add to welding machine operator's productivity.

Good luck

Gopal


From: 'b shekar' via Materials & Welding <materials-welding@googlegroups.com>
To: "materials-welding@googlegroups.com" <materials-welding@googlegroups.com>
Sent: Thursday, 11 December 2014 2:08 PM
Subject: [MW:22542] Re: Titanium tube welding and cooling time required

Dear Sirs,

What might be the temperature at the time of fusing the 0.7 mm thk tube by tungsten rod against the titanium tube sheet.
 
BVNR Sekhar

Senior Manager

Thermal Powertech Limited

Nellore, A.P.

Mob:+917680023063

sekhar.batlanki@tpcil.com 


From: b shekar <bvnrshekar@yahoo.co.in>
To: "materials-welding@googlegroups.com" <materials-welding@googlegroups.com>
Sent: Thursday, 11 December 2014 2:05 PM
Subject: Titanium tube welding and cooling time required

Dear Sir,

We have Titanium tube of Dia. 25*0.7 thk tubes for condenser. A titanium layer of 5mm upon the carbon steel plate on which these tubes were cut to surface size of 0.5 mm protruding, later expansion 5-6% of the 0.7 mm thk tube there by seal welding with orbital welding machine.

What i want to know is there any cooling time required for the tube to be welded and the heat dissipated on the main tube sheet requires any cooling by Air Conditioning or natural cooling. In the earlier projects of 9 units we have never used the AC but, in this project the QC asked to use AC.  I am worried of cracks and concern about using AC which immediately cools down the weld bead or titanium sheet resulting a cracks or repair.

kindly suggest me.  
 
BVNR Sekhar

Senior Manager

Thermal Powertech Limited

Nellore, A.P.

Mob:+917680023063

sekhar.batlanki@tpcil.com 


--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/d/optout.


Comments

Popular posts from this blog

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...

[MW:5202] RE: 5200] NDT after PWHT

------------------------------------- Interpretation:  I‑89‑14 Subject:         Section I (1986 Edition, 1987 Addenda), PW‑11,                  NDE Prior to PWHT Date Issued:     December 15, 1988 File:            BC88‑393   Question: Does PW‑11 require that NDE be performed on welds after they have been subjected to the postweld heat treatment required by PW‑39?   Reply: No, unless the conditions described in PW‑11.2.2 exist. ---------------------------------------------- Interpretation:  VIII-1-98-09 Subject:         Section VIII, Division 1 (1995 Edition, 1996 Addenda); NDE                 ...

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...