[MW:22547] random radiography in pipe line

Dear all,
in my project we are performing random radiography as per as per ASME 31.8 and cliend specification(saudiaramco). now the issue is when we performing random inspection which means radiography.
the following additional requirements also we need to follow as per saudi aramco.

16.7.1.4
When random radiography or ultrasonic testing is permitted
for onshore lines the percentage of radiography must be
increased if the repair rate is not below an acceptable level.
The extent of coverage (RAD) listed means the percentage
of welds completed that day that shall be inspected over
their entire length. The joints to be inspected shall be
selected to include a representative selection from all
welders. Additional emphasis may be placed on welders
with repair rates higher than the current job average.

16.7.1.5
The minimum extent of Radiographic or Ultrasonic testing
shall be in accordance with ASME B31.4 or ASME B31.8
as applicable. An increased percentage is required if a
higher percentage of coverage is established by either of the
following methods listed in 16.7.1.5.1 or 16.7.1.5.2 (both
methods shall be calculated and the higher percentage rate
shall govern).
16.7.1.5.1
Linear Basis
% RAD =
(N x D)
(318 x L)
(1)
where:
% RAD is the percent minimum radiographic
or ultrasonic coverage to be applied to the
production the following day.
L = total length of repairs, mm
N = total number of joints welded in one day
D = pipe diameter, mm

16.7.1.5.2
Joint Basis
The following repair rates are calculated on a
joint basis, i.e., the number of joints requiring
repairs divided by the total number of joints
inspected for that day's welds.
a) An increase to 50% RAD is required when
the repair rate exceeds 30%. This increase
shall be required for both the same day's
(i.e., additional joints must be inspected to
increase the RAD for that day to 50%) and
the next day's production.
b) An increase to 100% RAD is required
when the repair rate exceeds 50%.
This increase shall be required for both
the same day's (i.e., all other joints for
that day must be inspected) and the next
day's production.

now as per my under standing the above mentioned classes are if the repair percentage is not in acceptable level. then only we need to follow  as per class 16.7.1.4.

please give your valuable suggection.

Regards,
balaji

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/d/optout.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...