Skip to main content

RE: [MW:14678] RE: 14600] RE: USE of PQR of GTAW+SMAW for new WPS GTAW process only.

Yes they may be combined.  In this case the maximum base metal thickness will be governed by the most limiting qualified process thickness.  This can, as in this case, result in one process governing the lower bound and the other process governing the upper bound.

 

Since SMAW cannot be used to weld base metals with thickness less than 5mm, it is the lower bound for the combined WPS.

 

Since GTAW cannot be used to weld base metals with thickness greater than 16mm it is the upper bound for the combined WPS.

 

Hope this is clearer.

 

John A. Henning

Welding & Materials

 

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of sevak hiren
Sent: Saturday, June 23, 2012 12:27 AM
To: materials-welding@googlegroups.com
Subject: Re: [MW:14661] RE: 14600] RE: USE of PQR of GTAW+SMAW for new WPS GTAW process only.

 

Thanks a lot sir for this clarification.

 

I got most of the reviews that you can not combine two different welding process PQRs which are less than 13 mm thk, which is wrong assumption as per your clarification.

Futher I would like to ask this question.

 

Two different PQRs e.g. One GTAW Process only - Thk.8 mm & One SMAW Process only - Thk.12 mm (Both without impact test requirement)

 

Can these two PQRs be combined to creat One WPS for GTAW + SMAW ?

 

If yes then what will be the thk. range qualified for Base Metal ? 

 

Is it 1.5 To 24 mm OR 5 mm To 16 mm ?

 

Thanks once again in advance.


 

On Fri, Jun 22, 2012 at 10:06 PM, John Henning <jhenning@deltak.com> wrote:

Yes. These can be combined.  I assume that for both PQRs the base metal thickness was the same as the filler metal thickness, 8mm.

 

You then have a WPS qualified for base metal thickness (QW-451.1) 1.5mm to 16mm and each process qualified to a maximum deposit thickness of 16mm. 

 

Such a WPS could be convenient since the amount of GTAW and SAW within a joint that is 16mm or less is not limited.  At the extreme, the same WPS could be used to deposit the complete joint with GTAW or the entire joint could be done by SAW (assuming you have allowed for back gouging and back welding on the WPS).

 

 

John A. Henning

Welding & Materials

 

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of sevak hiren
Sent: Friday, June 22, 2012 8:03 AM
To: materials-welding@googlegroups.com
Subject: Re: [MW:14655] RE: 14600] RE: USE of PQR of GTAW+SMAW for new WPS GTAW process only.

 

Two different PQRs e.g. One GTAW Process only - Thk.8 mm & One SMAW Process only - Thk.8 mm 

 

Can these two PQRs be combined to creat One WPS for GTAW + SMAW ?

 

If yes then what will be the thk. range qualified ? 

 

Is it a must requirement as per Section IX that a minimum of 13mm must be welded with the root process in order to "ride along" with the fill process to the maximum that fill process is qualified for ?

On Wed, Jun 20, 2012 at 1:47 AM, John Henning <jhenning@deltak.com> wrote:

Mr. Mohammed-Al-Wi,

Respectfully, you response is incorrect for the situation described.  I believe Mr. Nakwal is asking if he can take a PQR performed with two process and split them into two separate WPS's, one for each process.  This can be done per the last paragraph of QW-200.4(a) which states;
"When following a WPS that has more than one welding process, filler metal or set of variables, each process filler metal, or set of variables may be used individually or in different combinations provided  (1) the essential, non-essential, and required supplementary essential variables associated with the process, filler metal, or set of variables are applied   (2) the base metal and deposited weld metal thickness limits of QW-451 for each process , filler metal, or set of variables are applied.

So, Mr. Nakwal has a PQR performed on base metal 8mm thick, with 3mm GTAW deposited metal and 5mm SMAW deposited metal.

Per QW451.1, it qualifies for GTAW:  Base metal thickness 1.5mm ~ 16mm, and deposited GTAW filler metal to a maximum of 6mm
And it qualifies for SMAW:  Base metal thickness 1.5mm ~ 16mm, and deposited SMAW filler metal to a maximum of 10mm

I suggest looking at Interpretations IX-78-47, IX-86-23 Q1 & Q2, IX-95-10, and IX-04-08.  In addition, you might want to look at Interpretations IX-81-32, IX-86-01 and IX92-97.

QW-200.4(b) applies only when trying to COMBINE two PQR's with into a single PQR, where a minimum of 13mm must be welded with the root process in order to "ride along" with the fill process to the maximum that fill process is qualified for.  An example would be a GTAW PQR with 13mm thickness combined with a SAW PQR with 38mm thickness to yield a WPS with a GTAW root and SAW fill qualified to for base metal thickness range of 5mm to 200mm.  The GTAW process in this example would be limited to a deposited thickness of 26mm.

Let me know if you have any questions.

John A. Henning
Welding & Materials

-----Original Message-----
From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of ahmraha@yahoo.com
Sent: Tuesday, June 19, 2012 8:39 AM
To: materials-welding@googlegroups.com
Subject: [MW:14600] RE: USE of PQR of GTAW+SMAW for new WPS GTAW process only.


-----Original Message-----
From: mohd
Sent:  15/06/2012, 9:53  am
To: Materials & Welding
Subject: [MW:14556] Re: USE of PQR of GTAW+SMAW for new WPS GTAW process only.


Dear all,

if you go through 200.4(b) For GTAW, SMAW, GMAW, PAW, and SAW, or combinations of these processes, a PQR for a process recording a test coupon that was at least 1⁄2 in. (13 mm) is required hence u cant creat two WPS.

Regrds,
Mohammed-AI-WI.



On Jun 11, 5:02 am, Parveen Kumar Nakwal <pknak...@gmail.com> wrote:
> Dear Experts,
>
> Can we use S.S to S.S 8mm base metal thickness PQR of GTAW (3mm)+SMAW
> (5mm) for the making for new WPS of S.S to S.S with GTAW only, with
> 2mm base metal thickness only ?
>
> Waiting for reply..
>
> Regards.
> Parveen K. Nakwal

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

______________________________________________________________________
The information in this email is confidential, and is intended solely for the addressee(s). If you are not the intended recipient of this email please let us know by reply and then delete it from your system; you should not copy this message or disclose its contents to anyone. The internet can not guarantee the integrity of this message. HAMON (and its subsidiaries) shall (will) not therefore be liable for the message if modified.
______________________________________________________________________

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.


______________________________________________________________________
The information in this email is confidential, and is intended solely for the addressee(s). If you are not the intended recipient of this email please let us know by reply and then delete it from your system; you should not copy this message or disclose its contents to anyone. The internet can not guarantee the integrity of this message. HAMON (and its subsidiaries) shall (will) not therefore be liable for the message if modified.
______________________________________________________________________

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.


______________________________________________________________________
The information in this email is confidential, and is intended solely for the addressee(s). If you are not the intended recipient of this email please let us know by reply and then delete it from your system; you should not copy this message or disclose its contents to anyone. The internet can not guarantee the integrity of this message. HAMON (and its subsidiaries) shall (will) not therefore be liable for the message if modified.
______________________________________________________________________

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...