Skip to main content

Re: [MW:14665] Impact WPS P1G1 to P1G1 &P1G2 to P1G2 Qualified P1G1 to P1G2 with impact ?

As per QW-403;

"If, however, two or more qualification records have the same essential and supplementary essential variables, except that the base metals are assigned to different Group Numbers within the same P-Number, then the combination of base metals is also qualified. In addition, when base metals of two different P-Number Group Number combinations are qualified using a single test coupon, that coupon qualifies the welding of those two P-Number Group Numbers to themselves as well as to each other using the variables qualified."


So the answer of Q1 is "No" and Q2 is "Yes".


Regards

Himan



On Sat, Jun 23, 2012 at 5:07 AM, Kavin202082 <kavin202082@yahoo.com> wrote:
Nope , u need to qualify P1 G1 to P1 G2 supplementry essential. Once u qualify tis It wil cover P1 G1 TO P1 G1, P1G2 TO P1 G2 AND P1G1 TO P1G2.Combination of g1 &g2 in one pqr req, nt combination of both pqr


Sent from Samsung Mobile


-------- Original message --------
Subject: Re: [MW:14647] Impact WPS P1G1 to P1G1 &P1G2 to P1G2 Qualified P1G1 to P1G2 with impact ?
From: samshuddin k <sam.renja@gmail.com>
To: materials-welding@googlegroups.com
CC:


1. No
2. Yes

On 6/22/12, mohd <mohd52100@gmail.com> wrote:
> Dear experts,
>
> Dear Expert,
>
> 1)Two PQR P1 G1 to P1 G1 & P1 G2 to P1 G2 with imapct, Qualified
>
>  WPS With Impact P1G1 to P1G2 Ans : Yes Or NO.
>
> 2) PQR P1G1 to P1G2 with Impact,Qualified Following WPS,
>
>    a) P1G1 to P1G1 with Imapact  Ans Yes Or NO
>    b) P1G2 to P1G2 with Impact   Ans Yes or No.
>
> I thinks these answer more clarified Mr lalit Querry.
>
> Thanks,
> Mohd.
>
>
> On Jun 21, 9:47 am, LALIT VADADORIYA <lalit.vadador...@gmail.com>
> wrote:
>> Dear expert,
>>
>> If welding procedure is qualified for the SA 516 Gr.60 to same (P No.1
>> Group 1 to same), then is it required to conduct another PQR for the SA
>> 516
>> Gr.70 to same (P No.1 Group 2 to same), if impact requirement is
>> applicable
>> for both material at same temperature?
>>
>> --
>> Regards
>>
>> *Lalit Vadadoriya
>> Sr.Engineer (Inspection)
>> Engineers India Limited*
>> *Dahej Petrochemical Complex,*
>> *Dahej (Gujarat)*
>
> --
> To post to this group, send email to materials-welding@googlegroups.com
> To unsubscribe from this group, send email to
> materials-welding+unsubscribe@googlegroups.com
> For more options, visit this group's bolg at
> http://materials-welding.blogspot.com/
> The views expressed/exchnaged in this group are members personel views and
> meant for educational purposes only, Users must take their own decisions
> w.r.t. applicable code/standard/contract documents.
>

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...