Re: [MW:29396] SA 333 Gr 6 Heat Treatment

Dear Ramin,

Very satisfied answer but I have another question regarding the use of A106 Instead of A333.

If available A106 Gr. B MTC is meeting the chemical requirements of A333 Gr.6 and pipe  is HOT FINNSED (HF), A106 doesn't required heat treatment in case of HF.

In this case A106 can be use only after impact testing or pipe must require heat treatment?


Regards,



On Wed, Mar 27, 2019 at 8:12 AM Ramin Kondori <raminkondori@gmail.com> wrote:
Dear Vikram:

First, you have to know what are the mechanisms which result in low-temperature impact characteristics.

A333 basically is a Carbon Steel (see chemical analysis requirements) which its impact toughness has been improved through reducing impurity levels plus a heat treatment. 

Here, of course, the steel making process is important to give you low impurity levels which means you'd better have killed steel and you would need more Mn% to extract Sulphur out and then, you apply a heat treatment to seal the deal. That's basically how A333 is made (there are some other things that manufacturers do but these are the basics).

I remember a project where we required LTCS pipes but we only had A106 instead (good quality) and due to new Iranian sanctions, we were not able to purchase A333 pipes we needed. We first, checked the chemical analysis of our A106 pipes (they met A333 chemical analysis requirements) and then sent them for heat treatment (and ordered required tests and surface treatments etc.) and we had our LTCS pipes. Of course, not every client approves this but our engineering justification was correct and we had almost no other choice.

So to answer your question, there are exceptions but yes, A333 normally requires heat treatment. 

Regards
Ramin  Kondori
Sr. QA/QC & Welding Engineer
-----------------------------------------------------------
PG-Dip. in Welding Engineering (IWE  AT  0070)
BSc. in Civil Engineering (IUT)
BGAS Painting Inspector
ASNT Level I&II
                        
IIW-Logo-Colour-small


On Wed, Mar 27, 2019 at 6:52 AM José Juan Jiménez Alejandro <jjjimeneza@gmail.com> wrote:
I recommend that you read the attached table, I hope you find it useful, the SA 333 Gr 6 is assigned a P1.  

El lun., 25 mar. 2019 a las 21:52, vikram saipogu (<saipoguvikram@gmail.com>) escribió:
Dear All,

Do SA 333 Gr 6 Pipe need Heat Treatment ?

*For Hot Finish Seamless Pipes

Best Regards,
Vikram Saipogu

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.


--

Ing. José Juan Jiménez Alejandro

ASME Independent Consultant 

and Technical Manager SSI-TPI

Cel. +52 812 352 4606

Skype: jjjimeneza

Twitter: @jjjimeneza



--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...