Not necessary. As you are performing the PWHT. Refer point 5 with my comments.

Btw you have necessary peening tools available? 

Thanks & regards
Sandeep Kumar

On Saturday, March 23, 2019 at 6:25:45 AM UTC+3, Josnit wrote:
Thanks for your reply, does weld require peening/hammering?

Sent from my iPhone

On Mar 22, 2019, at 23:52, sandeep kumar <sandeep...@gmail.com> wrote:

See my comments.

On Thursday, March 21, 2019 at 8:36:30 AM UTC+3, Josnit wrote:
Dear Experts,

We have observed a crack on a roller of material ZG35CrMo (34CrMo4). We want to do weld repair. Could you please advise the below;
1. Consumable to be used: Use E8018-B2
2. Preheat temperature: 150-200 Deg C & maintained during the welding.
3. Inter pass temperature: 250 Deg C max
4. Any post heating: No specific post heating required.
5. Final heat treatment temperature : U didnt specified the thickness & depth of the weld groove you will prepare for the repair. You can consider a temp of 725 Deg C for 2 hrs holding minimum. use a heating & cooling rate of 150 Deg C/ Hr and controlled heating-cooling above 350 Deg C.
6. Any special precautions?: Follow above instructions, it will be no issue.

Thanks & regards
Sandeep Kumar 
MSc. WE, IWE, Research fellow.

On Thursday, March 21, 2019 at 8:36:30 AM UTC+3, Josnit wrote:
Dear Experts,

We have observed a crack on a roller of material ZG35CrMo (34CrMo4). We want to do weld repair. Could you please advise the below;
1. Consumable to be used
2. Preheat temperature 
3. Inter pass temperature 
4. Any post heating
5. Final heat treatment temperature 
6. Any special precautions?

Sent from my iPhone

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...