Re: [MW:24559] Reg: combination of 2pqr's make a wps

Though asme ix permit combination of two pqs to make one wps, yet that does not mean that 2 pqr could be indiscriminately be combined. You can combine 2 pqr if there is overlap in essential and supplementary essential variables of the 2 pqr. For example the requires reduction of 55ºC as essential variable and increase of more than 55ºC in preheat as supplementary essential variable. 
If your case you pqr A preheat = 50ºC , then range qualified = 5- 105 and 
Pqr B preheat  = 170 , then range allowed = 115 - 225.
Since there is overlap between the two examples,  then both can not be combined. 
Note,  the figures stated above are just examples not real figures. 

Wilfred Kojo ( AWS CWEng )


On Sun, 20 Mar, 2016 at 7:35 am, Chandra
<chandrasekhar.palapala@gmail.com> wrote:
My thinking is QW-200.3(f) when impact test not require.
Must refer to QW-200.4(b) but reading that para, still confuses.
Could anyone suggest more???


Best Regards,
Chandra

On 19-Mar-2016, at 7:00 PM, Lalu Rajendran <lalucpt@gmail.com> wrote:

Hi,
please refer the below extract QW-200.3 (f), and hope this will suffice.

<image.png>

regards,
LALU

On Sat, Mar 19, 2016 at 3:29 PM, Chandra <chandrasekhar.palapala@gmail.com> wrote:
Dear to all,

I would like to ask you about the combination of pqr's

I have PQR A - 8mm (gtaw+smaw)
PQR B - 21.5mm (gtaw+smaw)
Both the pqr's were impact tested

now i want to make a wps using the 2pqr's as the thickness range 8mm to 43mm with impact requirements.

I require suggestions on this. Please give comments n valuable answers

Chandra
Welding Engineer


Best Regards,
Chandra

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/6F07097A-4544-4757-AC19-2334BE4464DD%40gmail.com.
For more options, visit https://groups.google.com/d/optout.

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAOwU13vj%3DhC8sfcUq2sj9GzPjdB79iz%3D0ze3N8UgW%3Dv5G4qBeA%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/51273241.2622925.1458458361537.JavaMail.yahoo%40mail.yahoo.com.
For more options, visit https://groups.google.com/d/optout.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Re: [MW:14950] RE: 14919] Stress relieving Rejected for 5 min less soaking time.

Dear All, I have been a CONSULTANT FOR such problem & my personal opinion is expressed as follow. I fully agree with views expressed so far. But bag to differ that " Code is a law, with engineering judgments. Hence the inspector has the rights to declare that the original HT was inadequate." Inspectors & total industry must resist the "REJECTION" . We as intellectual & having seniority must become practical. How the code will revise???. ANS.: One is experiments (Pure research) & second is such chances that gives opportunity to experiment !!! _______________________________________________________________________________________________ My understanding is that it is P1 material. In that case every pass normalizes the immediate bottom pass. Hence code requirement for P1 FOR MANDATORY SR is 32 mm & above thickness. SOLUTION:  In any case 0. After SR=PWHT no PTC testing is required as per code--Unless for low temp. vessels. That means code ...