Skip to main content

Re: [MW:24523] RE: 24509] Corrosion in CRA pipes

As per my understanding, in galvanic corrosion, material listed lower in galvanic table is the one which should deteriorate. In this case, cs is the lower grade and should deteriorate, not the alloy 825. 
In all carbon steel piping, gasket winding and inner rings is normally SS, but there is no issue of galvanic corrosion.
I think, this issue of contamination should require more discussion.

Regards,
Ahmed



On Sun, 13 Mar, 2016 at 12:29 pm, Alan Denney
<alan@denney1.freeserve.co.uk> wrote:

I understand that the designer has selected alloy 825 (as internal cladding) as adequate for the in-process service and you are asking why you have to remove swarf, from within the pipe. Since the swarf is from cutting a clad pipe it will be largely carbon steel. The reason is that the alloy 825 relies on a layer of passive surface scale to make it corrosion resistant. The swarf will set up a galvanic corrosion cell, assisted by the crevices formed under the corrosion product, the protective layer will be breached by the corrosion the surface will be pitted and corrosion can proceed in the pit regardless of what is done to the surface. I suggest you search for the terms, galvanic corrosion, pitting corrosion and crevice corrosion to understand the risks being created. The requirement that you prevent the ingress of swarf is correct.

 

Alan Denney

AKD Materials Consulting Ltd

 

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of berry gamaliel
Sent: 13 March 2016 03:17
To: materials-welding@googlegroups.com
Subject: [MW:24509] Corrosion in CRA pipes

 

Dear Experts 

 

In our project we are using CRA pipes, API 5L Grade B, thk- 35 mm. cladded with UNS00825  thk-5mm. 

 

Due to improper preservation of spools grinding and machining wastes deposited or setteled inside the spools and oxidation and corrosion started in a minor way. 

 

Please suggest whether chemical cleaning is required to to remove the minor corrosion or as it is a corrosion resistance alloy pipes will it withstand the corrosion. 

 

Another clarification too as it is a Corrosion resistance alloy why it cannot resist or prevent corrosion from grinding and machine wasted and during the service condition highly corrosive fluids will pass though it so how it will withstand that. 

 

Please clarify experts. 



--

Regards

 

 

Berry Gamaliel

 





--

Regards

 

 

Berry Gamaliel

 

 

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAKN5ewYsLRKgL0NyDp4_UYcQTBkiHk5ZF1-S--%2BbRmoup8Xukg%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/1908571874.492308.1457884345662.JavaMail.yahoo%40mail.yahoo.com.
For more options, visit https://groups.google.com/d/optout.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Re: [MW:14950] RE: 14919] Stress relieving Rejected for 5 min less soaking time.

Dear All, I have been a CONSULTANT FOR such problem & my personal opinion is expressed as follow. I fully agree with views expressed so far. But bag to differ that " Code is a law, with engineering judgments. Hence the inspector has the rights to declare that the original HT was inadequate." Inspectors & total industry must resist the "REJECTION" . We as intellectual & having seniority must become practical. How the code will revise???. ANS.: One is experiments (Pure research) & second is such chances that gives opportunity to experiment !!! _______________________________________________________________________________________________ My understanding is that it is P1 material. In that case every pass normalizes the immediate bottom pass. Hence code requirement for P1 FOR MANDATORY SR is 32 mm & above thickness. SOLUTION:  In any case 0. After SR=PWHT no PTC testing is required as per code--Unless for low temp. vessels. That means code ...