Re: [MW:23262] De hydrogenition heat treatment for 5Cr material

Hi Mr. Biju,

With due respect to all the experts comments, My question is how you qualified your procedure,  the same should be followed through out the project. Did you not considered the spec while establishing procedure.

I agree with the comment that it's a non essential variable. But WPS has to be revised.


Thanks & regards,

Jay Poojary
QA/QC Engineer,
OCLLC,  Nigeria

On Aug 3, 2015 7:27 PM, "'james gerald' via Materials & Welding" <materials-welding@googlegroups.com> wrote:
 Not Required.  The reason for dehydrogenation treatment by raising the temperature to 250-300 degC is that hydrogen atoms are mobile and have more diffusivity which will drive the hydrogen out of the weldment depending on holding time 1-3 hours.

Not a good practice to avoid dehydrogenation treatment. In this case since PWHT was done immediately, it would have resulted in diffusion of hydrogen from the weldment and thus avoids delayed cracking.

Since this is a client specification violation, may be taking a RT after 48 hours may be a chance to convince the client.


 
Thanks & Regards
J.Gerald Jayakumar
0091-9344954677


From: Kannayeram Gnanapandithan <kgpandithan@gmail.com>
To: materials-welding <materials-welding@googlegroups.com>
Sent: Monday, August 3, 2015 5:45 PM
Subject: Re: [MW:23258] De hydrogenition heat treatment for 5Cr material

not required and it is not essential variable, since pwht is taken immediately after completion of weld is more than enough 

THANKS & BEST REGARDS,
KG.PANDITHAN, IWE,  AWS-CWI, CSWIP 3.1,
CONSULTANT-WELDING & QUALITY



On Mon, Aug 3, 2015 at 2:48 PM, shanmuganathan .subbiah <shanmuganathan.subbiah@gmail.com> wrote:
Dear 
It is not acceptable , Post heat shall be carried as per approved WPS

On Mon, Aug 3, 2015 at 8:01 AM, biju <biju.psl@gmail.com> wrote:
Our client spec. requires 5Cr material with thickness more than 10mm requires dehydrogenition heat treatmnet 
But the contractor has welded and immediately completed PWHT without going for DHT, Is that acceptable
--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
Visit this group at http://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/6c6af4e1-2a5b-4a8f-9aab-993accc61023%40googlegroups.com.
For more options, visit https://groups.google.com/d/optout.



--
Regards
SHANMUGANATHAN SUBBIAH
AIB- Vincotte International & Partners LLC
PO.Box-420, PC -116
MAF, Sultanate of Oman
Tel: +968 24565771
Fax: +968 24565772
Mob: +968 92096714
--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
Visit this group at http://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAD2bsBR-xgN%3DdEpFipj-O-nBy7XiSJdNxgbDHe%3D0HpyKMxBfUw%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.

--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
Visit this group at http://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAJzm4eNbe4Z8_OymmxaKrNi-sxdJH0x6ssTjaJu4vnjXvEe_Qw%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.


--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
Visit this group at http://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/1815740217.889169.1438609392513.JavaMail.yahoo%40mail.yahoo.com.
For more options, visit https://groups.google.com/d/optout.

--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
Visit this group at http://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAAcO%3DyTL1%2Ba%3D636dqaxUeaZ6%2BftfpKbLViRE3B-nq8EynPLJDg%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...