Re: [MW:19303] MECHANICAL TESTING OF SA 266 GR 2

Dear Mr. sinha,

I am confused over interpretation of code because in both clause it is Forgings so i have to consider all forgings or a forging for weight calculation.

Regards,
Ankit Gandhi

On Tuesday, 19 November 2013 10:05:48 UTC+5:30, sina wrote:
Dear friend,
One tensile test will be sufficient. Just care about the location of sampling.

Regards


On Mon, Nov 18, 2013 at 8:20 PM, Ankit Gandhi <asgan...@gmail.com> wrote:
Dear Expert,

Delvery Condition is Normalized
Heat No. & Lot No. is same
Qty. 4 Nos.
Weight:1500 Kg / Forging

How many testing is required as per Section II P-A?

8.2.1.1 For forgings weighing 5000 lb [2250 kg]
or less at the time of heat treatment, one tension test shall
be taken from one forging per heat in each heat–treatment
charge. When heat treatment is performed in continuoustype
furnaces with suitable temperature controls and
equipped with recording pyrometers so that complete heattreatment
records are available, a tempering charge may
be considered as any continuous run not exceeding an 8 h
period.

8.2.1.2 For forgings and forged bars weighing over
5000 lb [2250 kg] at the time of heat treatment, one tension
test shall be taken from each forging.

Regards,
Ankit Gandhi

--
To post to this group, send email to material...@googlegroups.com
To unsubscribe from this group, send email to materials-weld...@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.



--
M. Shokri Arfaei
ISA-ISTS - Metallurgy Lab. Manager
ASNT NDT Level III
International Welding Engineer

Tel.: +98 21 66282127
Fax: +98 21 66282779
Mob.:+98 912 1394023





On Tuesday, 19 November 2013 10:05:48 UTC+5:30, sina wrote:
Dear friend,
One tensile test will be sufficient. Just care about the location of sampling.

Regards


On Mon, Nov 18, 2013 at 8:20 PM, Ankit Gandhi <asgan...@gmail.com> wrote:
Dear Expert,

Delvery Condition is Normalized
Heat No. & Lot No. is same
Qty. 4 Nos.
Weight:1500 Kg / Forging

How many testing is required as per Section II P-A?

8.2.1.1 For forgings weighing 5000 lb [2250 kg]
or less at the time of heat treatment, one tension test shall
be taken from one forging per heat in each heat–treatment
charge. When heat treatment is performed in continuoustype
furnaces with suitable temperature controls and
equipped with recording pyrometers so that complete heattreatment
records are available, a tempering charge may
be considered as any continuous run not exceeding an 8 h
period.

8.2.1.2 For forgings and forged bars weighing over
5000 lb [2250 kg] at the time of heat treatment, one tension
test shall be taken from each forging.

Regards,
Ankit Gandhi

--
To post to this group, send email to material...@googlegroups.com
To unsubscribe from this group, send email to materials-weld...@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.



--
M. Shokri Arfaei
ISA-ISTS - Metallurgy Lab. Manager
ASNT NDT Level III
International Welding Engineer

Tel.: +98 21 66282127
Fax: +98 21 66282779
Mob.:+98 912 1394023




--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.

Comments

Popular posts from this blog

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...

[MW:5202] RE: 5200] NDT after PWHT

------------------------------------- Interpretation:  I‑89‑14 Subject:         Section I (1986 Edition, 1987 Addenda), PW‑11,                  NDE Prior to PWHT Date Issued:     December 15, 1988 File:            BC88‑393   Question: Does PW‑11 require that NDE be performed on welds after they have been subjected to the postweld heat treatment required by PW‑39?   Reply: No, unless the conditions described in PW‑11.2.2 exist. ---------------------------------------------- Interpretation:  VIII-1-98-09 Subject:         Section VIII, Division 1 (1995 Edition, 1996 Addenda); NDE                 ...

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...