Skip to main content

Re: [MW:18789] Multiple process GTAW+SMAW Process,

E7018 is not to be used in DCSP


On Fri, Sep 27, 2013 at 5:30 AM, Saravanan Sornam <saravanshyla@gmail.com> wrote:
Dear Mr.Sridhar ,

Thank you for your details .

As ASME II C, SFA 5.1, Table 1 and I referred other major welding consumable manufacturer's catalogues ,  E7018 is not recommended for DCEN ( Straight Polarity ), so practically you might have achieved with DCEN for E7018 on pipes with full penetration.

Have you tested any tensile, bend tests in PQR with the same technique you have mentioned in your mail .

If it is OK, then I would check in my shop too.

Regards,
Saravanan.


On Thu, Sep 26, 2013 at 7:19 PM, c sridhar <sridhar305@yahoo.com> wrote:

There is  no doubt about  penetration(medium)  level with E 7018 & E 7016 type electrodes compared to E 6010.

But what I have said is " E 7018 gives full penetration  with DC EP & both E 7018 & E 7016 electrodes give deep
penetration with DC SP " and could be used for root application.

The penetration depth  is  comparable to welds made with E 6010 using  DC RP.
Filler & Cap passes to be done with DC RP.

Sridhar.
 

From: kannayeram gnanapandithan <kgpandithan@gmail.com>
To: materials-welding <materials-welding@googlegroups.com>
Sent: Thursday, 26 September 2013 10:55 AM
Subject: Re: [MW:18770] Multiple process GTAW+SMAW Process,

7016&7018 will give medium penetration unlike 6010 which gives deep penetration


On Tue, Sep 24, 2013 at 11:17 PM, c sridhar <sridhar305@yahoo.com> wrote:
E7018 type electrodes give radiographic quality  full penetration welds on single 'v' groove butt joints with DC EP .

Both E 7016 & E 7018 type electrodes give deep  and full penetration welds with DC EN 
(like in E 6010) and filler
passes to be continued with DCEP.

Both techniques were adopted successfully in pipe line joints.

sridhar.





From: "george.dilintas@gr.bureauveritas.com" <george.dilintas@gr.bureauveritas.com>
To: materials-welding@googlegroups.com
Sent: Wednesday, 18 September 2013 12:53 PM
Subject: Re: [MW:18690] Multiple process GTAW+SMAW Process,

If you want to involve only SMAW then E-6010 is the only option for the root pass.
For filling you could continue with E-7018

rudolf saldanha ---17/09/2013 10:30:00---hI, Saravanan,  

From: rudolf saldanha <rudolf_jude@yahoo.com>
To: "materials-welding@googlegroups.com" <materials-welding@googlegroups.com>
Date: 17/09/2013 10:30
Subject: Re: [MW:18673] Multiple process GTAW+SMAW Process,
Sent by: materials-welding@googlegroups.com




hI, Saravanan,
 
May I know if it is mandatory by code that back gouging has to be done when we have a Full Penetration Joint using only SMAW process.
As far as I know, backing and back gouging are supplementary essentials for SMAW process.
 
To get a full penetration it is not compulsory to go for GTAW + SMAW process, but we can still do it with SMAW only.
 
We can use LB52U which also belongs to SFA 5.1 just as E7018, and it is commonly used for welding on pipelines where welding is done on one side.
 
http://www.weldingsupply.com.au/index.php/kobe-lb52u-low-hydrogen.html
 
The above link may be of help.
 
Please correct me if I am wrong.
 
Thanks and regards
Rudolf
 
 
 

From: Saravanan Sornam <saravanshyla@gmail.com>
To:
 materials-welding@googlegroups.com
Sent:
 Tuesday, 17 September 2013, 14:05
Subject:
 Re: [MW:18670] Multiple process GTAW+SMAW Process,

Hi San ,

I said that , only SMAW on the Inaccessible Pipe size, for example 6 ", cannot be welded and even you cannot get Full Penetration using E7018 only on Single V Bevel.

It should be welded only by using GTAW for Root and subsequent welds by SMAW until Cap.

Regards,
Saravanan,
Korea


On Mon, Sep 16, 2013 at 7:32 PM, jaffar ali riyas mohamed nizamin <jaffarqc1987@gmail.com> wrote:
--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at
http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm

The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit
https://groups.google.com/groups/opt_out.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at
http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm

The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit
https://groups.google.com/groups/opt_out.
This message contains confidential information. To know more, please click on the following link: http://disclaimer.bureauveritas.com
--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.


--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.


--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...