Re: [MW:13467] RE: 13441] NDE FOR BUTT WELD

You can perform  PT for surface and RT & UT for subsurface .......
 
RT by placing the cut film on to the available area ( chances of missing HAZ region on one side)
UT by using Longitudinal Shear wave probes and normal probes ( weld shall be flush ground to ensure full coverage ) for subsurface and below surface
PT for surface
 
 
Best  Regards
Venu Moturu
 

From: "george.dilintas@gr.bureauveritas.com" <george.dilintas@gr.bureauveritas.com>
To: materials-welding <materials-welding@googlegroups.com>
Sent: Wednesday, 11 January 2012, 19:25
Subject: Re: [MW:13454] RE: 13441] NDE FOR BUTT WELD

Since it is a austenitic SS UT may not be possible. It is not possible to form a tapered transition 1:3 as required by almost all ASME code sections, which would make RT easier?
Best regards
Dr Georgios Dilintas
Authorized Nuclear Inspector
Authorized Inspector Supervisor
HBS Regional Technical Manager
  From: "Desai Jignesh (Mumbai - Piping)" [J.J.Desai@ticb.com]
  Sent: 10/01/2012 18:06 ZE5B
  To: "materials-welding@googlegroups.com" <materials-welding@googlegroups.com>
  Subject: RE: [MW:13448] RE: 13441] NDE FOR BUTT WELD

It is a butt weld.
 
It is welding of SS 321 forged component (Nozzle) of bevel end with 90 el. Actually forged nozzle is without tapering.
Proper radiography is executed for the BW valves joints as shown in Photo-0060.
 
UT is also a problem since probe movement is possible at only one side (Towards elbow) and there is no inside access.
 
It is 100% Radiography lines with high pressure – 1500#.
 
Regds/Jignesh
 
From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of vijayan
Sent: 10 January 2012 16:18
To: materials-welding@googlegroups.com
Subject: [MW:13444] RE: 13441] NDE FOR BUTT WELD
 
Hi
 
What is the joint configuration
BR
M.Vijayan
 
From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of Desai Jignesh (Mumbai - Piping)
Sent: Tuesday, January 10, 2012 12:58 PM
To: materials-welding@googlegroups.com
Subject: [MW:13441] NDE FOR BUTT WELD
 
Can somebody write me about the possibility of either radiography OR Ultrasonic testing of attached butt weld?
 
We have tried to carry out radiography with and without non metallic support as in the attached snaps but image is not clear.
 
Regds/Jignesh

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
 
This communication and any files transmitted with it are confidential and may also be privileged. It is for the exclusive use of the intended recipient(s). If you are not the intended recipient or the person responsible for delivering it to the intended recipient(s), please note that any form of distribution, copying or use of this communication or information contained in it is strictly prohibited and may be unlawful. If you have received this communication in error please return it to the sender, and delete the material from any computer. We reserve the right to monitor email communications through normal internal and external networks. We believe but not warrant that the email and the attachments are virus free. The statement and opinions expressed in this communication are those of the writer and do not necessarily represent those of Madina Group, whose registered office address is

P.O. Box 20459, Doha, Qatar.
Tel. +974 44600818
Fax. +974 44603143
--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~
NOTICE: This message contains information which is confidential and the copyright of our company or a third party. If you are not the intended recipient of this message please delete it and destroy all copies. If you
are the intended recipient of this message you should not disclose or distribute this message to third parties without the consent of our company. Our company does not represent, warrant and/or guarantee that the integrity of this message has been maintained nor that the communication is free of virus, interception or interference. The liability of our company is limited by our General Conditions of Services.
Nota : Ce message contient des informations confidentielles propriété de notre société et/ou d'un tiers. Si vous n'êtes pas parmi les destinataires désignés de ce message, merci de l'effacer ainsi que toutes ses copies. Si vous êtes parmi les destinataires désignés de ce message, prière de ne pas le divulguer ni de le transmettre à des tiers sans l'accord de notre société. Notre société ne peut garantir que l'intégrité de ce message a été préservée ni que la présente communication est sans virus, interception ou interférence. La responsabilité de notre société est limitée par nos Conditions Générales de Services.
~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~
--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.


Comments

Popular posts from this blog

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...

[MW:5202] RE: 5200] NDT after PWHT

------------------------------------- Interpretation:  I‑89‑14 Subject:         Section I (1986 Edition, 1987 Addenda), PW‑11,                  NDE Prior to PWHT Date Issued:     December 15, 1988 File:            BC88‑393   Question: Does PW‑11 require that NDE be performed on welds after they have been subjected to the postweld heat treatment required by PW‑39?   Reply: No, unless the conditions described in PW‑11.2.2 exist. ---------------------------------------------- Interpretation:  VIII-1-98-09 Subject:         Section VIII, Division 1 (1995 Edition, 1996 Addenda); NDE                 ...

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...