Re: [MW:13468] amendment for this WPS regarding

Hi,
As per QW406.1 and 406.3,Preheat temperature and Interpass temperature shall be specified on the WPS. 
Option-1:
What is the Preheat and Interpass temperature recorded on the PQR? If you didn't do preheat while doing PQR,you can revise the WPS as ambient and Interpass temeprature as maximum recorded on the PQR. Since it is dissimilar joint, it shall not be more than 175 degrees(Maximum).
Option-2:
If you did preheat while doing PQR, your WPS shall be specified the Preheat Temp.For example if you Did or  plan to do preheat of 150degrees on PQR,your WPS shall be specified as 95degrees(Minimum). Because as per QW-406.1 A decrease of more than 100°F (55°C) in the preheat temperature qualified is an essential variable.Also you can specify Interpass temeprature as maximum recorded on the PQR but it shall not be more than 175 degrees(Maximum).
 
Thanks & Regards,

(Karthik)

Karthikeyan.S
QA/QC Manager
German-Thai Boiler Engineering Cooperation Limited.
Rayong Factory ;
379 Moo.6 Soi 8, Tambol Pananikom,
Nikompattana, Rayong 21180 THAILAND
Tel : +66 38 897 035-9 Ext. 137
Fax : +66 38 897 034
Hand Phone: 0066 892512282


From: venkateswaran k <kvnkat@rediffmail.com>
To: materials-welding@googlegroups.com
Sent: Thursday, January 12, 2012 3:25 PM
Subject: [MW:13460] amendment for this WPS regarding

Dear All,

We qualified WPS for Material SA 516(P:1,G:1) TO SA240TP 316L(P:8,G:1) by SMAW process as per ASME Sec IX ,thickness range- base metal Grove is: 5 -30 mm,Filler metal:E309 Mol.

My question is while qualifying we did not mentioned Preheating and Inter pass temperature (in WPS -QW 406),now one of our client asking for these two parameters need to be filled /required, in this case how to convince him. Whether can I make amendment for this WPS, it is acceptable as per ASME Sec IX. If yes can u provide format for this amendment.

kvr
Follow Rediff Deal ho jaye! to get exciting offers in your city everyday.
--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.


Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...