Skip to main content

Re: [MW:13501] RE: 13484] Pre-heating for cutting

For carbon steels upto certain thickness it is not required.

Only when the thickness is very high and for Chrome-moly steels it is recommended to preheat the base material before cutting to avoid formation of undesirable phases which leads to cracking. Preheating before cutting will result in grain coarsening and impair the Impact properties.

Moreover it is always recommended to grind the HAZ of the Gas cut surfaces.
 
Thanks & Regards

J.Gerald Jayakumar
0091-9344954677

From: DEBASISH <debasish.uae@gmail.com>
To: materials-welding@googlegroups.com
Sent: Wednesday, January 18, 2012 1:08 PM
Subject: Re: [MW:13500] RE: 13484] Pre-heating for cutting

Perfect. To add more on this:
Basically this becomes more and more stringent, in case of low temp. steels, wherein the grain coarsening is detrimental to it's Impact ( Toughness ) properties. Also, Preheating before flame cutting is required to decrease the thermal gradient which eventually decreases the chances of grain coarsening & also reduces thermal shock or any initiation of micro fissuries leading to cracks latter. Workshop remedy is: we ask to remove the HAZ formed by flame cutting,  by grinding the skin of the flame cut edge preparation.  Offcourse, This stringent practice is generally not required for general Mild steels grades of steel.
regars,
DEBASISH
Dubai
+971504349936.
 
 
 
 
 
On Tue, Jan 17, 2012 at 2:35 PM, sandeep monody <smv.monody@gmail.com> wrote:
Dear all,
 
 
The purposes of preheat are to avoid crack due to sudden heating and for wide heat affected zone,so in my openion preheating is required for both cutting and welding.
 
Regards,
 
Sandeep.M.V
 


 
On Tue, Jan 17, 2012 at 10:31 AM, Lakshman Kumar.B <lakshmankumar4@gmail.com> wrote:
Dear All,
 Beyond all the technical aspects, small logic for this situation….
This is only my view…
 
After cutting the edges are again welding to some part / connection(say pipe, fitting, flange, etc or leaving like that) in all the cases if welding is going to do it will be again preheat and PWHT after welding so any thermal shocks will be relived during PH, PWHT,
 
So I think no need of pre heating.
 
Thanks and Regards................?
 
Lakshman Kumar.B|Manager |Lanco Infratech Limited
Plot No 1255 | Sanjeevani chowk | Mahanadi vihar | Cuttack 753004
Phone : + 91 671 2445033 | Mobile : +91 9937286851 |www.lancogroup.com
Go Green|The future will thank you
 
 
From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of jesti fer
Sent: Monday, January 16, 2012 3:22 PM

To: materials-welding@googlegroups.com
Subject: [MW:13484] Pre-heating for cutting
 
Dear Experts,
 
I need your help for this subject, We are fabricating some piping as per B31.3, the material ASTM A106 Gr.B, 8"Sch-XXS and 160 and we are doing preheat and PWHT for welding, but my enquiry pre heat is required for cutting also? It is mentioned in any code or any other were? Please help me
 
Jesti
--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.


Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...