Skip to main content

Re: [MW:7172] Wearing of plasite paint

Hi,

It might be happened due to poor surface preparation , while blasting
blasting not respected the parameters. skin temperature might less
than dew point or after more laps of time sweep blast not done before
painting.

solution only you have to re-blast properly and repaint.


On 9/23/10, Qamlr <qamlr@cicb-chemicon.com> wrote:
> Dear All
>
> We have received feed back from customer that HP & LP Shell of the
> compressor, have hade complete disintegration of plasite coating and
> excessive rust formation in the shell . An excessive plasite wearing has
> been noticed on the shell
>
> We have used plasite 7156 and conformed as per the specification called
> during painting in house
>
> Could experts give feed back for such failure and cause for the same?. We
> shall have to take corrective action
>
> Thanks
>
> Regards
>
> Prashanth Hegde
>
> ________________________________
> Please don't print this e-mail unless you really need to.
> *******************************************************************
> This e-mail is confidential. It may also be legally privileged. If you are
> not the addressee you may not copy, forward, disclose or use any part of it.
> If you have received this message in error, please delete it and all copies
> from your system and notify the sender immediately by return e-mail.
> Internet communications cannot be guaranteed to be timely, secure, error or
> virus-free. The sender does not accept liability for any errors or
> omissions.
> *******************************************************************
> "SAVE PAPER - THINK BEFORE YOU PRINT!"
>
> --
> To post to this group, send email to materials-welding@googlegroups.com
> To unsubscribe from this group, send email to
> materials-welding-unsubscribe@googlegroups.com
> For more options, visit this group's bolg at
> http://materials-welding.blogspot.com/
> The views expressed/exchnaged in this group are members personel views and
> meant for educational purposes only, Users must take their own decisions
> w.r.t. applicable code/standard/contract documents.
>


--
Dear


Thanking you.

With Warm Regards,

Muthu Barathi P
mobile : 09967300544
mobile: 09022848735

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...