Dear all,

From production point of view, electrodes with  higher deposition rates are being considered. But when it comes to quality, hydrogen induced cracking to be considered, hence basic coated electrodes  are the best.

Still cellulose electrodes r being considered, have a control on preheat temp on pipe, if req as per code and baking of electrodes, to reduce the possibility of hydrogen.

Note: hydrogen in excess of 4ml / kg is prone to hydrogen induced cracking.

Regards,
Ram

From: Demir Alp ILIKOBA
Sent: ‎17-‎10-‎2015 02:06 PM
To: materials-welding@googlegroups.com
Subject: Re: [MW:23728] Cellulosic Electrode Usage Instead of Basic Electrode

Dear Sir;

I know i can't change 7018 to 7010 depending on same PQR thus i am also making preparation for a new PQR. So please take my question as application will be done on new PQR. Additonally i shall say their intention to use cellulosic electrodes on large pipes (i.e 96'').Your comments are appreciated.

Best Regards;

Demir

On Sat, Oct 17, 2015 at 1:21 PM, Perumal Govindan <perumalgovindan@gmail.com> wrote:

Hi

You can not replace the electrode, since SFA number, UTS & alloying element presence to meet the weld metal properties  and WPS (approved) for pipe welding.

Regards
PG

On 17 Oct 2015 11:51, "Demir Alp" <demiralp85@gmail.com> wrote:
  • Dear Sirs;

    I would like to get Your professional advisory regarding selection of the filler material in Piping Welding of the P:1 G:1 Pipe Materials.

    For a large variety of Thickness and Diameters i have written 3 different WPS by combination of GTAW + SMAW process with usage of ER 70S-6 (Root and Hot Passes using GTAW) and E7018 (for Fill passes and Cap using  SMAW process.)

    However Our construction dept , insists on usage of Cellulosic electrodes instead of basic electrodes for higher deposition rate.

    As QA/QC I am doubtful replacing 7018 with 7010 or any other cellulosic electrode because of their tendency for hydrogen induced cracking. I'd like to add in my previous project We used to have X70 pipes and our employer didn't allow us to use cellulosic elecrodes just because hydrogen induced cracking.

    Thus I would like  to get your professional opinion regarding this subject,

     Best Regards; 
    Demir


--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
Visit this group at http://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/4783eb1a-1cc3-41df-8a2e-9700b07dc15b%40googlegroups.com.
For more options, visit https://groups.google.com/d/optout.

--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
Visit this group at http://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CANiuf9fUf-DEFKzGiM4S3HM6TWqdrn8Q-wd4DBf%2BdkBiNJNo0A%40mail.gmail.com.

For more options, visit https://groups.google.com/d/optout.

--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
Visit this group at http://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CACj12PB5oc77hCyd3YYn8ZKswWM4de%3D4O3n1%2BpBg7YG0UHq8ng%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.

Comments

Popular posts from this blog

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...

[MW:5202] RE: 5200] NDT after PWHT

------------------------------------- Interpretation:  I‑89‑14 Subject:         Section I (1986 Edition, 1987 Addenda), PW‑11,                  NDE Prior to PWHT Date Issued:     December 15, 1988 File:            BC88‑393   Question: Does PW‑11 require that NDE be performed on welds after they have been subjected to the postweld heat treatment required by PW‑39?   Reply: No, unless the conditions described in PW‑11.2.2 exist. ---------------------------------------------- Interpretation:  VIII-1-98-09 Subject:         Section VIII, Division 1 (1995 Edition, 1996 Addenda); NDE                 ...

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...