Skip to main content

RE: [MW:23760] RE: 10970] heat input calculation

Below is a link to a calculator that will calculate Kj to C.

Hope this helps

http://www.convertunits.com/from/kilojoules/to/celsius+heat+unit

 

Best Regards

 

Jim Price | Welding Engineer, CWI

Direct:  320.7463439 | Fax: 417-862-5564

jimprice@polarcorp.com

 

 

 

 

 

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of Joshi Gaurang
Sent: Tuesday, October 20, 2015 4:03 AM
To: Materials & Welding
Cc: kathalingam.qaqc@ppl.com.sg
Subject: Re: [MW:23759] RE: 10970] heat input calculation

 

Hi,

 

What i should consider, that heat input is v*I*n*60/TS, TS is travel speed so it will give me Kj/mm but how i can convert it to temperature ....

Additionally now i can convert it into temperature than it will give me input heat but what about actual heat inut which may very metal by metal so how i can calculate that .

 

Thank you 

On Sunday, 8 May 2011 17:24:04 UTC-7, Kathalingam Babu wrote:

Hi

 

The arc efficiency as mentioned below is used for the actual heat input calculation.

 

The stds/Codes works on the theoretical HI , which is more than the actual HI, so no need to worry about the arc efficiency factor.

 

Infact the those values are only the approximate values , if you want actual arc efficiency values you have to go for an calorimeter set up to find out the actual one

 

Thanks & Regards,

 

K. Babu

----- Original Message -----

From: Pieper QSI

Sent: Friday, May 06, 2011 6:07 PM

Subject: RE: [MW:10980] RE: 10970] heat input calculation

 

Correct me when I'm wrong but this efficiency factor is not mentioned in any original calculation formula and specifications such as ASME section IX and/or EN ISO 15609/15614 therefore in my opinion cannot taken into account for official calculation of Heat Input.

 

Met vriendelijke groeten / Best Regards

 

Herman Pieper

 

Pieper Quality Support & Inspection

Phone: +31 (0)521 380083

Fax:     +31 (0)84 7539225

Cell:     +31 (0)6 51691215

www.pieper-qsi.nl

 

Van: material...@googlegroups.com [mailto:material...@googlegroups.com] Namens Fitria Rahman
Verzonden: vrijdag 6 mei 2011 10:48
Aan: material...@googlegroups.com
Onderwerp: Re: [MW:10979] RE: 10970] heat input calculation

 

Dear All

i notice that there is an important piece of formula is missing. the heat input formula given by Firman shall be multiplied by efficiency which is depending on its welding process. GMAW & SAW having efficiency 0.9, GTAW=0.8, SMAW=0,75

rgds

2011/5/6 muthusrinivasan muthuselvam <msm...@gmail.com>

conversion factor to convert the travel time to mm/sec

 

On Fri, May 6, 2011 at 1:46 PM, Martin Prad <marti...@hotmail.com> wrote:

what is 60 (V*I*60) in this formula?
 


From: vinod....@blissanand.com
To: material...@googlegroups.com
Subject: [MW:10974] RE: 10970] heat input calculation
Date: Fri, 6 May 2011 13:00:05 +0530

You can calculate by using following formula:-

 

Heat Input = (V*I*60)/(Travel Speed in mm) this will come in J for KJ please further devide it with 1000.

 

For the below value the Heat Input shall be

0.50 KJ.

 

With kind regards,

Vinod Kumar Kataria

GM - Operations

Bliss Anand Private Limited,

92B/93B Sector 5

IMT Manesar,Gurgaon,

National Capital Region Delhi.

India .

Phone : +91-124-4366000 (9 Lines)

Mobile Phone : +91-9560199004

Fax : +91-124-2290884

 

From: material...@googlegroups.com [mailto:material...@googlegroups.com] On Behalf Of Martin Prad
Sent: Friday, May 06, 2011 11:00 AM
To: material...@googlegroups.com
Subject: [MW:10970] heat input calculation

 

gents,
 
how to calculate the heat input in KJ/mm if i have got the folowing parameters?
 
Amperage=71
Voltage=9.5
Travel speed=3.2 inch/minute
can you please put these in the formula?
 
thanks.

--
To post to this group, send email to material...@googlegroups.com
To unsubscribe from this group, send email to materials-weld...@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.


--
To post to this group, send email to material...@googlegroups.com
To unsubscribe from this group, send email to materials-weld...@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to material...@googlegroups.com
To unsubscribe from this group, send email to materials-weld...@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

 

--
To post to this group, send email to material...@googlegroups.com
To unsubscribe from this group, send email to materials-weld...@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

 

--
To post to this group, send email to material...@googlegroups.com
To unsubscribe from this group, send email to materials-weld...@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to material...@googlegroups.com
To unsubscribe from this group, send email to materials-weld...@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
Visit this group at http://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/b4a14ae0-2f1e-460d-9150-a1bf5c7eb2b3%40googlegroups.com.
For more options, visit https://groups.google.com/d/optout.

Comments

Popular posts from this blog

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...

[MW:5202] RE: 5200] NDT after PWHT

------------------------------------- Interpretation:  I‑89‑14 Subject:         Section I (1986 Edition, 1987 Addenda), PW‑11,                  NDE Prior to PWHT Date Issued:     December 15, 1988 File:            BC88‑393   Question: Does PW‑11 require that NDE be performed on welds after they have been subjected to the postweld heat treatment required by PW‑39?   Reply: No, unless the conditions described in PW‑11.2.2 exist. ---------------------------------------------- Interpretation:  VIII-1-98-09 Subject:         Section VIII, Division 1 (1995 Edition, 1996 Addenda); NDE                 ...

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...