RE: [MW:23719] Impact test- minimum thk requirement

Hi DV George

The charpy requirements starts from 5 mm and above. Below 5 mm is not required as per ASTM A370  which is Standard Test Methods and Definitions for Mechanical Testing of Steel Products page 5 Note 7 2003 publication.  

On the other hand example 5 section 7 in EEMUA 153 which is SUPPLEMENT TO ASME B31.3 states as follows: 

"""""7 BS 3603, Charpy V-notch impact testing at low temperature BS 3603 : 1991 Sec. 12.2.3 states that impact testing shall not be carried out on tubes less than 6 mm thick. For the particular example in which a nominal wall thickness of 5.6 mm is specified, impact testing will not be carried out. However impact values may be assumed as those given for thicker material supplied to the same specification. """"" 

Also most of project specifications don't require charpy test below 6 mm.  Hence, in your case the impact test is not required. I think this clarifies your doubt.  

Best regards Elshan.

________________________________
> Date: Thu, 15 Oct 2015 12:11:43 +0400
> Subject: Re: [MW:23717] Impact test- minimum thk requirement
> From: harishkannepalli@gmail.com
> To: materials-welding@googlegroups.com
>
> For this diameter and thickness, it is not possible to perform impact test.
>
> 2013-05-22 14:33 GMT+04:00 victor george
> <dvgeorge@gmail.com<mailto:dvgeorge@gmail.com>>:
> Hi Experts,
>
> Please explain what is the minimum thickness requirement of impact test.
>
> Material: A790 S31803 pipe
> Size: 1/2' Sch 80 (WT- 3.73mm)
> Sour service
>
>
> Question: Is it possible to do impact test on 3.73 thk?
>
>
> Best Regards,
> DV.George
>
>
> --
> To post to this group, send email to
> materials-welding@googlegroups.com<mailto:materials-welding@googlegroups.com>
> To unsubscribe from this group, send email to
> materials-welding+unsubscribe@googlegroups.com<mailto:materials-welding%2Bunsubscribe@googlegroups.com>
> For more options, visit this group's bolg at
> http://materials-welding.blogspot.com/
> http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
>
> The views expressed/exchnaged in this group are members personel views
> and meant for educational purposes only, Users must take their own
> decisions w.r.t. applicable code/standard/contract documents.
> ---
> You received this message because you are subscribed to the Google
> Groups "Materials & Welding" group.
> To unsubscribe from this group and stop receiving emails from it, send
> an email to
> materials-welding+unsubscribe@googlegroups.com<mailto:materials-welding%2Bunsubscribe@googlegroups.com>.
> For more options, visit https://groups.google.com/groups/opt_out.
>
>
>
>
>
> --
> Regards,
> Mr. Harish.
>
> --
> You received this message because you are subscribed to the Google
> Groups "Materials & Welding" group.
> To unsubscribe from this group and stop receiving emails from it, send
> an email to
> materials-welding+unsubscribe@googlegroups.com<mailto:materials-welding+unsubscribe@googlegroups.com>.
> To post to this group, send email to
> materials-welding@googlegroups.com<mailto:materials-welding@googlegroups.com>.
> Visit this group at http://groups.google.com/group/materials-welding.
> To view this discussion on the web visit
> https://groups.google.com/d/msgid/materials-welding/CAE4SttGWP4%3DOmSDzBUdE40NphU_M-FFBnRoNcOWJth%3D77G7JxA%40mail.gmail.com<https://groups.google.com/d/msgid/materials-welding/CAE4SttGWP4%3DOmSDzBUdE40NphU_M-FFBnRoNcOWJth%3D77G7JxA%40mail.gmail.com?utm_medium=email&utm_source=footer>.
> For more options, visit https://groups.google.com/d/optout.

Comments

Popular posts from this blog

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...

[MW:5202] RE: 5200] NDT after PWHT

------------------------------------- Interpretation:  I‑89‑14 Subject:         Section I (1986 Edition, 1987 Addenda), PW‑11,                  NDE Prior to PWHT Date Issued:     December 15, 1988 File:            BC88‑393   Question: Does PW‑11 require that NDE be performed on welds after they have been subjected to the postweld heat treatment required by PW‑39?   Reply: No, unless the conditions described in PW‑11.2.2 exist. ---------------------------------------------- Interpretation:  VIII-1-98-09 Subject:         Section VIII, Division 1 (1995 Edition, 1996 Addenda); NDE                 ...

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...