Re: [MW:30729] BASE METAL THIKNESS FOR PQR

Since you mention about range I assumed you are qualifying Wps for the range X60 - X65.

If it is a Joint between X60 - X65. then u can use the PQR for X65.

Thanks & Regards

J.Gerald Jayakumar




On Friday, April 10, 2020, 10:21:31 AM GMT+7, QA/QC <adnanziad49@gmail.com> wrote:


THANKS MASTER FROM YOUR ADVISE NOW ITS CLEAR  100/100 AS U MENTION BEFORE FROM YOUR EMAILS 

Le jeudi 9 avril 2020 13:05:04 UTC+2, gerr...@yahoo.com a écrit :
Instead of being confused, first you should know what is your Job.

Then the design  Code ASME B 31.4 or ASME B31.8


Snap shot provided below for you to decide.

Inline image



Inline image


See below requirement and snap shot of ASME B 31.8

Inline image


Thanks & Regards

J.Gerald Jayakumar




On Thursday, April 9, 2020, 05:00:52 PM GMT+7, QA/QC <adnan...@gmail.com> wrote:


IM CONFUSED , NORMALLY WHAT I SHOULD TO USE ASME 9 OR API 1104  

Le jeudi 9 avril 2020 07:02:56 UTC+2, gerr...@yahoo.com a écrit :
By below mail was based on API 1104 Code which considers yield strength as essential variable.

From your below mail I understand you are using ASME Sec.IX (correct me of I am wrong).

Acc to ASME Sec.IX one PQR is sufficient for API 5L X60 - X65 as they both fall under P1 Gr.2.

Acc to ASME Sec.IX thickness range qualified is 1.5mm to 15.84mm

Thanks & Regards

J.Gerald Jayakumar




On Thursday, April 9, 2020, 11:23:55 AM GMT+7, QA/QC <adnan...@gmail.com> wrote:


tnx for your reply 

So its mean that i should prepare two different Test coupon or what 

and for the maximum thikness of base metal from QW 451.1 THEY MENTION THAT  T QUALIFIED X 2  ITS MEAN 7.92 X2 = 15.84 mm


Le mercredi 8 avril 2020 13:52:38 UTC+2, gerr...@yahoo.com a écrit :
Considering Pipeline, API 1104 code was considered for below.

1. One PQR for X60 material
2. Another PQR for X65 material to be qualified'

If you qualify PQR on 6 inch wall thickness 7.92 mm then it qualifies from wall thickness 4.8mm to 19.1mm and no Limitation on Diameter

Thanks & Regards

J.Gerald Jayakumar




On Wednesday, April 8, 2020, 03:10:03 PM GMT+7, QA/QC <adnan...@gmail.com> wrote:


Hello 

i want to prepare a WPS for pipeline work with base metal API 5L X60 - X65  SMAW 

for the test coupon i want to use 6" with thickness = 7.92 mm 

want to know the minimum and maximum range for size and thickness used for the PQR 

BEST REGARDS

--
https://materials-welding. blogspot.com/
https://www.linkedin.com/ groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to material...@ googlegroups.com.

--
https://materials-welding. blogspot.com/
https://www.linkedin.com/ groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to material...@ googlegroups.com.
To view this discussion on the web visit
https://groups.google.com/d/ msgid/materials-welding/ 94cc40bc-2a64-4a7c-828d- 034cc090d77b%40googlegroups. com
.

--
https://materials-welding. blogspot.com/
https://www.linkedin.com/ groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to material...@ googlegroups.com.
To view this discussion on the web visit
https://groups.google.com/d/ msgid/materials-welding/ acc75da4-18b3-44c6-9398- 91d01641143b%40googlegroups. com
.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit
https://groups.google.com/d/msgid/materials-welding/88a400b1-f05d-48b0-acc5-c3b2b611ce45%40googlegroups.com
.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...