Re: Re: [MW:28774] Groove weld qualification for fillet weld

Dear Mohamed,
It depends on if impact test is required or no regardless if the qualification is done by fillet weld or groove weld so if you qualify by pure fillet weld or by groove welds, nothing changes because the thickness limitations are based on the impact test requirements, not on the method of qualification. The reason is that for impact requirements, we have to be very careful about the amount of welding and heat input then we have to limit the thickness as per QW-403.6 in ASME IX.
I hope it is clear now.

Thanks & Regards
Hisham Al. Mohammad
Welding Engineer & QA/QC Engineer
Mob: +971 56 433 7326 & +971 52 667 9935

On Sun, Dec 16, 2018 at 7:46 AM muneebslsa@gmail.com <muneebslsa@gmail.com> wrote:
Boxbe This message is eligible for Automatic Cleanup! (muneebslsa@gmail.com) Add cleanup rule | More info
Thats great and agreed, as clause 451.4s note very clearly stipulated as applied for notch. 

Anyhow i wonder if i would like to make a pure fillet weld qualifications as per QW-451.3, in this case i do not have any project butt welds requirement for production, but only fillets and limited  by the service case i need to do impact, what would you recommend on this scenario.

Please advise.


Regards,
Mohamed Muneeb Mahaboob
CSWIP 3.2-89247/2 
IRCA-9001:2015 LA
ASNT-NDT-L2-RTFI-RT-UT-MT-PT.
SAP#:70021650 APs:JAPID, QCS & QCI.
E muneebslsa@gmail.com M +91-636-955-7189
''If you know any art by any means then SCULPT IT - no matter how cheap or useless it is - JUST SCULPT IT, you will never know when experts will be on demand'' 
 
Date: 2018-12-15 12:22
Subject: Re: [MW:28769] Groove weld qualification for fillet weld
Dear All,
Table 451.4 states that: "Supplementary essential variables apply when toughness is required by other Sections" and by referring to QW-403.6, we will find that the thickness is limited in general not only for the groove weld. It means that fillet welds are including otherwise why this note regarding the supplementary essential variables is mentioned in QW-451.4 ?!
The groove welds govern fillet welds not vice versa.

On Monday, January 3, 2011 at 7:34:46 AM UTC+4, manpreet singh wrote:
Dear Pravin,

Usually I don't get to see many fillet weld qualifications since my current project is pipeline, but this specific case is for BARRED TEES, where Groove weld PQR was used for Fillet weld WPS, though all variables were satisfactory but I was not comfortable with QW-451.4 which says that any groove weld shall qualify for ALL Fillet welds,

Thanks for your time and also would like to request other members to look through the matter and give a sound reply.

Regards
Manpreet Singh


On Sat, 01 Jan 2011 13:43:32 , praveen alavandar <prave...@yahoo.com> wrote
Manpreet,
 
Please provide details of the production fillet weld configuration for more details.
Either clause QW 451.1 or QW 451.4 doesnt impose any additional restriction on thickness by referring QW 403.6 in it.
However QW 403.6 looks to be stand alone reference on limiting the base material thickness range.
This can be a good question to be answered by Sec.IX committee through interpretations, I dont know if there is any existing interpretation available for this case.
 
members can help it here.
 
What does your Authorised INspector say about this? In the mean while i'll also check with my Authorised INspector.
 
Regards,
 
A.Praveen 

--- On Thu, 12/30/10, manpreet <manpre...@rediffmail.com> wrote:

From: manpreet <manpre...@rediffmail.com>
Subject: Re: [MW:9014] Groove weld qualification for fillet weld
To: "material...@googlegroups.com" <material...@googlegroups.com>
Date: Thursday, December 30, 2010, 2:27 PM

Dear Pravin,

Perhaps i couldn't explain it properly,

For a production fillet weld joint between 25mm and 13mm thks, Can I use any groove weld PQR for making WPS without considering QW-451.1 and QW-403.6 ? 

Please answer me with code reference..

Regards
Manpreet Singh




On Thu, 30 Dec 2010 13:42:40 , praveen alavandar <prave...@yahoo.com> wrote
Manpreet,
 
There is not any catch point in Sec.IX to limit your fillet weld material thickness or weld deposit thickness even when impact testing is applicable.
 
You have to just follow QW 451.3 limits only.
 
Why is that you qualified a fillet PQR for an impact tested application, instead of supporting any groove weld PQR?
 
Regards,
 
A.Praveen

--- On Thu, 12/30/10, manpreet <manpre...@rediffmail.com> wrote:

From: manpreet <manpre...@rediffmail.com>
Subject: Re: [MW:9011] Groove weld qualification for fillet weld
To: "material...@googlegroups.com" <material...@googlegroups.com>
Date: Thursday, December 30, 2010, 12:37 PM

Dear Jaspal,

QW-403.6 is applicable for minimum base metal limits for impact tested qualification, What i m asking is that, QW-451.4 is stating that a groove weld qualification shall be qualified for all thickness of fillet weld, does that mean, we need not to follow QW-451.1 & QW-403.6....  

Somebody please answer this query......

Regards
Manpreet Singh
 


On Thu, 30 Dec 2010 10:47:24 +0530 JASPAL SINGH wrote
>Dear Manpreet,
>
>For Welder Qualification as per Section IX there is no variable for
>Impact . As far as base metal is concerend the only variable is 403.16
>& 403.18 in case of SMAW.
>
>As per below extract from ASME Section IX:
>
>QW-303.1 Groove Welds —General. Welders and welding operators who
>pass the required tests for groove
>welds in the test positions of table QW-461.9 shall be qualified for
>the positions of groove welds and fillet welds
>shown in table QW-461.9. In addition, welders and welding operators
>who pass the required tests for groove welds
>shall also be qualified to make fillet welds in all thicknesses and
>pipe diameters of any size within the limits of the
>welding variables of QW-350 or QW-360, as applicable
>
>Best Regards,
>
>JASPAL SINGH CWI-AWS, CSWIP-3.1
>ISGEC-PED, Yamunanagar, Haryana (India) PH: +911732307251 ;Mob.
>+918930111441(CUG), +919996624244
>www.isgec.com
>
>On Dec 30, 7:54 am, "manpreet " <manpreetsi...@rediffmail.com> wrote:
>> Dear All,According to QW-451.4, Groove weld qualifies for all thickness ranges of fillet welds,In production a a fillet joint with 25mm &amp; 13mm, impact test required,Is the code saying that QW-403.6 &amp; QW-451.1 will not be applicable here? Please give me your views.....RegardsManpreet Singh
>
>--
>To post to this group, send email to material...@googlegroups.com
>To unsubscribe from this group, send email to materials-weld...@googlegroups.com
>For more options, visit this group's bolg at http://materials-welding.blogspot.com/
>The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
>
--
To post to this group, send email to material...@googlegroups.com
To unsubscribe from this group, send email to materials-weld...@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to material...@googlegroups.com
To unsubscribe from this group, send email to materials-weld...@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to material...@googlegroups.com
To unsubscribe from this group, send email to materials-weld...@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to material...@googlegroups.com
To unsubscribe from this group, send email to materials-weld...@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.


--

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...