Re: [MW:28768] Welder Qualification

Dear Muneeb thanks for your reply.

Further to your reply if I refer the figure 3 it is a butt weld test piece so we are qualifying the fillet weld by butt weld 

What does the term supplemtary fillet weld test piece stands for .

Please clarify 


On Sat, Dec 15, 2018, 8:16 AM muneebslsa@gmail.com <muneebslsa@gmail.com wrote:
e) Butt welds may qualify fillet welds if a supplementary fillet weld test piece (see Figure 3) is welded with each process, filler material (FM) group and electrode covering/core, in accordance with Tables 3, 4, and 5. 

Reply: your fillet weld needs a supplementary qualifications as per ISO standards, where as in most codes - your fillet gets qualified with butt which is not here. 
so here you have to place a test piece as same as of FIGURE 3, to qualify a fillet, that too it has stated ''MAY'' which again MAY requires client or owners approval,  and it qualifies in accordance with table 3, 4 and 5, 
EX: you qualify with FM1 is qualified with 1 and 2 or you qualify with FM 5 only qualified for FM 5, same for rest. 
Table 3 — Range of qualification for filler material
Table 4 — Range of qualification for covered electrodes
Table 5 — Range of qualification for filler material types

The test piece shall be at least 10 mm thick, or the thickness of the butt weld test piece if the thickness is less, and completed using a single layer in the PB position. For this supplementary test, 

Reply: So you shall have 10mm thickness for fillet as minimum or least minimum as same as BUTT coupon if it is most least, for ex if butt is 9mm you shall use 9mm, PB-HORIZONTAL, position shall be completed with single layer.

the welder shall be qualified for all fillet welds as given for the butt weld qualification variables related to the range of qualification for fillet welds (e.g. Tables 7, 8, 9, 10 and 12). Fillet weld positions 
PA and PB are qualified by this test.

Reply: again table 7,8,9,10 and 12 qualification range given butt welds are as same for fillet, PA and PB flat and horizontal of fillets positions qualified through this butt weld positions.

Hope there is a clarity.

Thanks.


Regards,
Mohamed Muneeb Mahaboob
CSWIP 3.2-89247/2 
IRCA-9001:2015 LA
ASNT-NDT-L2-RTFI-RT-UT-MT-PT.
SAP#:70021650 APs:JAPID, QCS & QCI.
E muneebslsa@gmail.com M +91-636-955-7189
 
Date: 2018-12-14 17:38
Subject: [MW:28764] Welder Qualification
Dear friends need your help to clarify the highlighted point (e). 

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...