On Tue, Dec 4, 2018, 1:41 PM riaz rafeeque <riaz.rafeeque@gmail.com wrote:
Thanks for replies, 



We are following EIL specification , and API 1104.  This is natural gas pipeline of API 5L x 70, 6.62 mm. We deployed auto welding machine of PIPE WELDING TECHNOLOGY ITALY. 

During PQT , we observed that the root backing strip of Copper fused with Root run.  We are using GMAW process , with argon and Co2 gas mixture. Root 40 % CO2.  Filler wire ER 80S-D2

Attaching here few pics of same.


Me assuming few things based on discussion with site rep on Pipe Welding Technology , 

1) High Current or excess penetration. 

2) High Flowrate, or Density Caused by high percentage of CO2 led to high penetration.

3) Small root face. Currently it is 2 mm. 

4) Also someone suggested that 0.5mm of ID bevel may avoid root penetration and can eliminate fusion with copper backing strip. 


I need you guys help for resolving issue . Thank to all for responses so far.


Riaz Rafeeque






On Tue, Dec 4, 2018 at 12:43 PM muneebslsa@gmail.com <muneebslsa@gmail.com> wrote:
Hi,

Please confirm whether you incorporated below requirements,

Check para 328.3.2 WBM, (b) says If two abutting surfaces are to be welded to a third member used as a backing ring and one or two of the three members are ferritic and the other member or members are austenitic, the satisfactory use of such materials shall be demonstrated by welding procedure qualified as required by para. 328.2.

or

(c) Nonferrous and Nonmetallic Backing Rings. Backing rings of nonferrous or nonmetallic material may be used, provided the designer approves their use and the welding procedure using them is qualifiedas required by para. 328.2.

I had a same similar observation in my previous projects where like 500 welds were completed with SS backing strip which is a longitudinal welds of full encirclement, so not to get puncture with the base materials they have used SS plate backing strip removable without procedure qualifications, still i found some fusion / depostion in the backing and they said it is temporary, BM is CS BS is SS, so i made a violation, but you know it went in different level.

Anyhow even if you are working for SA projects, even tempeory backing strips shall be of same materials, please confirm whether you on SA projects? and did you demonstrate procedure qualification or your designer approved?


Thanks.


Regards,
Mohamed Muneeb Mahaboob
CSWIP 3.2-89247/2 
ASNT-NDT-L2-RTFI-RT-UT-MT-PT.
SAP#:70021650 APs:JAPID, QCS & QCI.
E muneebslsa@gmail.com M +91-636-955-7189

(6:8) They say, "Why has no ˹visible˺ angel come with him?" Had We sent down an angel, the matter would have certainly been settled ˹at once˺, and they would have never been given more time ˹to repent˺.

 
From: Ri@z
Date: 2018-12-04 11:14
Subject: [MW:28719] Auto Welding Copper back up strip fused with Root run
Dear All, 


We are introduced auto welding on 6.62 MM thickness , API 5L X 70 .  J groove prepared with 2 mm root face and zero root opening. 


Root has supported with copper back up strip/Shoes


But after welding we observed that copper back up strip is melted and fused with root run. 


Kindly help to resolve the issue. What are the possible reason for the problem ?? 


With Regards

Riaz Rafeeque 

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to a topic in the Google Groups "Materials & Welding" group.
To unsubscribe from this topic, visit https://groups.google.com/d/topic/materials-welding/kjXye15frFA/unsubscribe.
To unsubscribe from this group and all its topics, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...