Skip to main content

Re: [MW:27014] Re: Radiography acceptance criteria.

Mr. Dominic,

Thanks for your feedback.I will add your  suggestion on next revision.





On 19-Nov-2017 4:36 PM, "Dominic v.k.dominic" <v.k.dominic@gmail.com> wrote:
​Dear Pradip,
Thank you for the excel table and your time.
Please note that API-1104 Some of defect/flaw contractors will accepted reference of your table.
The API-1104 code allowed the range of below defects/flaws,
Lack of fusion - up to 25mm in (300 mm) length of weld.
Lack of penetration - up to 25mm (300 mm) length of weld.
Undercut - up to 50mm (300 mm) length of weld.

Kindly refer the code and please take your account in next version.

Thanks,
Best Regards,

Dominic V.K.




On 19 November 2017 at 11:17, Engineer Inam-Ul-Haq <engrhaq673@hotmail.com> wrote:

Very Nice, Mr. Pradeep Ghosh




From: materials-welding@googlegroups.com <materials-welding@googlegroups.com> on behalf of Pradip Ghosh <pradipg2@gmail.com>
Sent: Sunday, November 19, 2017 11:59 AM
To: materials-welding@googlegroups.com
Subject: Re: [MW:27011] Re: Radiography acceptance criteria.
 
 Dear ,Shashank C Vagal  use bellow link to download the file.

https://drive.google.com/open?id=0ByvRBXye0uymdW9aekp1M0J1cHc

On Fri, Nov 17, 2017 at 11:49 AM, 'Shashank Vagal' via Materials & Welding <materials-welding@googlegroups.com> wrote:
Dear Pradeep Ghosh,
Please fwd to me a copy of this excel program .
 
Thankfully Yours,
Shashank C Vagal  
301, PRATHAMESH, M G Rd – Mahant Rd, Vile Parle East, Mumbai 400 057 INDIA
 


On Friday, 17 November 2017 9:15 AM, SULTAN <sultanhyder0@gmail.com> wrote:


Very Nice effort  Mr.Goshi
i think one thing is missing in this is ASME Sec.I

Thanks,

Regard's
Sultan 
QC Engineer 
MEC Engineering

On Thursday, September 5, 2013 at 3:18:52 PM UTC+5, Pradip Ghosh wrote:
Dear All,

I have prepared a excel program in which you can find Radiography acceptance criteria of ASME Sec IX,API-650,API-1104,ANSI B 31.3 and ASME Sec VII Div  in a click.
Please give me your review and comments.




Pradip Ghosh

QA/QC Engineer
Mott MacDonald (P) Ltd.
--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.


--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to a topic in the Google Groups "Materials & Welding" group.
To unsubscribe from this topic, visit https://groups.google.com/d/topic/materials-welding/k5wvDu0g8dU/unsubscribe.
To unsubscribe from this group and all its topics, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.



--
Thanks and Regards,

Pradip Ghosh
QA/QC Engineer
Mott MacDonald (P) Ltd

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to a topic in the Google Groups "Materials & Welding" group.
To unsubscribe from this topic, visit https://groups.google.com/d/topic/materials-welding/k5wvDu0g8dU/unsubscribe.
To unsubscribe from this group and all its topics, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...