RE: [MW:27049] Welding after PWHT on SA335 P11 coil

Per Table UCD-56-4 of Section VIII, Division 1 of the ASME BPVC (for ASME P-No. 4 steels):

1.       For butt welds in pressure barriers, PWHT is required for thicknesses greater than 5/8-inch (16-mm)

2.       For non-pressure attachment fillet welds, PWHT is required for thicknesses greater than 1/2-inch (13-mm)

 

Per Table 132.2 of ASME B31.1 (for ASME P-No. 4 steels):

1.       For butt, groove, & socket welds in pressure barriers, PWHT is required for pipe thicknesses greater than 5/8-inch (16-mm)

2.       For non-pressure attachment fillet welds, PWHT is required for pipe thicknesses greater than 5/8-inch and fillet throat thicknesses greater than 1/2-inch (13-mm)

 

Per Table 132.2 of ASME B31.3 (for ASME P-No. 4 steels):

1.       For butt, groove, & socket welds in pressure barriers, PWHT is required for pipe thicknesses greater than 5/8-inch (16-mm)

2.       For non-pressure attachment fillet welds, PWHT is required for pipe thicknesses greater than 5/8-inch and fillet throat thicknesses greater than 1/2-inch (13-mm)

 

D. Thompson

 

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of jitendra raghuwanshi
Sent: Thursday, November 23, 2017 5:49 AM
To: materials-welding@googlegroups.com
Subject: Re: [MW:27045] Welding after PWHT on SA335 P11 coil

 

As per my knowledege alloy materials of grade P11 & P12 doesnt require pwht if thickness is less than 13mm.

 

On 22 Nov 2017 5:28 pm, "Hareesh K V" <hareesh13h@gmail.com> wrote:

Sir,

 

With proper approvals and procedure you can go for local PWHT.

 

Regards,

 

Hareesh K V

 

On Nov 22, 2017 5:11 PM, "Makrand Sakpal" <makrands9@gmail.com> wrote:

Dears,

 

We have ordered fired heater in which coil material is SA335 P11. Coil size is 6" x SCH 40 (i.e. 6.625" OD x 0.28" THK). These coils are PWHT'd. Issue is, our vendor forgot to weld the thermocouple RF pads on the coil before PWHT. What needs to be done further if we weld the RF Pads on the already PWHT'd coils? Do we need to do PWHT again for that particular joint?

 

Please let us know your opinions.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

 

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...