Skip to main content

[MW:27070] RE: 27062] Welding of PLATES STRENX 700

Hi Hani,

 

Please see the attached datasheet for your reference. It's the data sheet from the OEM. It's not clear from your email, what's the thickness to be welded. However welding with 100 Ksi (UTS) welding consumable would be challenging, cracking may occur for any unspecified reasons.

 

Also use the welding products of reputed vendors. Also ask for diffusible hydrogen test results and the CE values of the welds (equal or less than the BM),so as  to minimize cracking while welding. This is in addition to application  of preheat and control of interpass" temperature.

 

Note these steels are of very high tensile steel, hence application of  preheat and control of interpass temperature has to selectively decided , upon consultation with the OEM and consumable vendors.

 

Thanks,

 

 

P.Goswami.P.Eng, IWE.

Welding & Metallurgical Specialist

Linkedin: https://www.linkedin.com/in/pradip-goswami-2999855/

Email:pgoswami@quickclic.net,pradip.goswami@gmail.com

 

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of Hani Al Masry
Sent: November 28, 2017 5:32 AM
To: materials-welding@googlegroups.com
Subject: [MW:27062] Welding of PLATES STRENX 700

 

Dear All

 

please advice welding of STRENX 700 with CS S275 and with it self 

 

attached MTC for your reference 

 

Regards,

H.A 

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.


Virus-free. www.avg.com

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...