Skip to main content

RE: [MW:14958] RE: 14919] Stress relieving Rejected for 5 min less soaking time.

UCS-56(b) “. . . The holding time at temperature as specified in Table UCS-56 need not be continuous.  It may be an accumulation of time of multiple postweld heat treatment cycles.”

 

John A. Henning

Welding & Materials

 

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of Ahmed Husain
Sent: Wednesday, July 25, 2012 5:10 AM
To: materials-welding@googlegroups.com
Subject: Re: [MW:14956] RE: 14919] Stress relieving Rejected for 5 min less soaking time.

 

Dear Mr. Pradip,

 

As per your below e-mail, PWHT time is cumulative. Is there any reference to support this? If you have , can you please e-mail.

 

Thanks and regards,

 

Ahmed Husain

From: Chetan Kapadia <cbkapadia@yahoo.co.in>
To: "materials-welding@googlegroups.com" <materials-welding@googlegroups.com>; mohd <mohd52100@gmail.com>
Cc: "pgoswami@quickclic.net" <pgoswami@quickclic.net>; "pgoswami@sympatico.ca" <pgoswami@sympatico.ca>
Sent: Tuesday, July 24, 2012 6:42 PM
Subject: Re: [MW:14950] RE: 14919] Stress relieving Rejected for 5 min less soaking time.

 

Dear All,

 

I have been a CONSULTANT FOR such problem & my personal opinion is expressed as follow.

 

I fully agree with views expressed so far.

 

But bag to differ that " Code is a law, with engineering judgments. Hence the inspector has the rights to declare that the original HT was inadequate."

 

Inspectors & total industry must resist the "REJECTION". We as intellectual & having seniority must become practical.

 

How the code will revise???.

 

ANS.: One is experiments (Pure research) & second is such chances that gives opportunity to experiment !!!

_______________________________________________________________________________________________

 

My understanding is that it is P1 material.

 

In that case every pass normalizes the immediate bottom pass.

Hence code requirement for P1 FOR MANDATORY SR is 32 mm & above thickness.

 

SOLUTION: 

 

In any case

 

0. After SR=PWHT no PTC testing is required as per code--Unless for low temp. vessels. That means code is assuming     that if every care is taken as per code then there is not much of a change in mechanical properties of WELD & HAZ.     Hence this minor time difference can not result in tremendous non agreeable metallurgical & OR mechanical OR         process guarantee type defect. Depending up on final use the best decision can be arrived at.

 

1.if sufficient length is available ON PRODUCT then carry out all DT.

 

2.if sufficient length is not available on product carry out HARDNESS survey on PP, HAZ & WELD.

   THIS WILL GIVE FAIR IDEA OF TT & WELD TENSILE VALUES. If + then proceed for all test on PTC.

 

3. Prepare additional Test piece & let it undergo simulated SR with less by 5 minutes. Test for all test required by

    product designed use.Prove with guts.Nothing goes wrong. 

 

Even if all above proves wrong accept the defeat with guts on experimenting.

 

Please do it even for your self satisfaction.  Who knows It might become a code case.

 

How can we have code without negative tolerance on time: Whatsoever--???.

 

All this is without any prejudice to the contribution by other experts in the group. Further comments welcome for better understanding on the issue.

 

Best Regards,
C.B.KAPADIA
Free-Lance Fabrication Technology & API Monogram Certification consultant

 

From: pgoswami <pgoswami@quickclic.net>
To: materials-welding@googlegroups.com
Sent: Tuesday, 24 July 2012 5:42 PM
Subject: RE: [MW:14949] RE: 14919] Stress relieving Rejected for 5 min less soaking time.

 

Harish/Mohd,

 

I am not trying to act as moderator.

 

Looking at the problem, a separate simulation may be as time consuming as the original HT. Code is a law, with engineering judgments. Hence the inspector has the rights to declare that the original HT was inadequate. The simplest solution what looks to me is to perform additional SR for 15-20 mins and satisfy code requirements.

 

PWHT time is all cumulative , and there no restriction form ASME code.

 

Thanks.

 

Pradip Goswami,P.Eng.IWE

Welding & Metallurgical Specialist

Ontario , Canada .

Email-pgoswami@sympatico.ca,

pgoswami@quickclic.net

 

 

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of Harish Kannepalli
Sent: Monday, July 23, 2012 11:58 AM
To: materials-welding@googlegroups.com
Subject: Re: [MW:14942] RE: 14919] Stress relieving Rejected for 5 min less soaking time.

You can propose the following to your client:

            Perform Simulation on separate coupon, check the mechanical & metallurgical properties. If they meet the code requirements, it may be acceptable. After all, code is made by humans for humans.

2012/7/23 John Henning <jhenning@deltak.com>

Most common materials require 1 hour/25mm or 60minutes/25mm and I assume you are working with one of these materials.  Then, for a 40mm thick material the required minimum soak time is (40mm)*(60min.)/(25mm) = 96 minutes

 

You don’t meet Code required minimum soak time.  Your soak time must exceed the minimum time.  Therefore, your pipe weld is unacceptable.  No discussion – it is clearly unacceptable in its present condition.

 

John A. Henning

Welding & Materials

 

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of mohd
Sent: Saturday, July 21, 2012 1:52 AM
To: materials-welding@googlegroups.com
Subject: [MW:14919] Stress relieving Rejected for 5 min less soaking time.

 

Dear expert,

 

As per ASME 8-1-UCS-56

 

We have done SR for our 40mm thk-30" pipe joint.

 

but unfortunetly, soaking time was just short by 5min.Now our client/PMC both are not agree to release.

 

Required time : 1hr.15min

Actual Time : 1hr.10min

 

It is acceptable OR could you share any technical view to convince client?

 

regards,

mohd.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.


______________________________________________________________________
The information in this email is confidential, and is intended solely for the addressee(s). If you are not the intended recipient of this email please let us know by reply and then delete it from your system; you should not copy this message or disclose its contents to anyone. The internet can not guarantee the integrity of this message. HAMON (and its subsidiaries) shall (will) not therefore be liable for the message if modified.
______________________________________________________________________

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to mailto:materials-welding%2Bunsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.



 

--

regards,

Harish.

 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.


______________________________________________________________________
The information in this email is confidential, and is intended solely for the addressee(s). If you are not the intended recipient of this email please let us know by reply and then delete it from your system; you should not copy this message or disclose its contents to anyone. The internet can not guarantee the integrity of this message. HAMON (and its subsidiaries) shall (will) not therefore be liable for the message if modified.
______________________________________________________________________

Comments

Popular posts from this blog

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...

[MW:5202] RE: 5200] NDT after PWHT

------------------------------------- Interpretation:  I‑89‑14 Subject:         Section I (1986 Edition, 1987 Addenda), PW‑11,                  NDE Prior to PWHT Date Issued:     December 15, 1988 File:            BC88‑393   Question: Does PW‑11 require that NDE be performed on welds after they have been subjected to the postweld heat treatment required by PW‑39?   Reply: No, unless the conditions described in PW‑11.2.2 exist. ---------------------------------------------- Interpretation:  VIII-1-98-09 Subject:         Section VIII, Division 1 (1995 Edition, 1996 Addenda); NDE                 ...

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...