Skip to main content

Re: [MW:14976] Need WPS clarification with ASME and EN

ASME: remember that Group No is supplementary essential parameter. So the PQR, in case impact test is required needs to be repeated. A no is an essential parameter which is very frequently forgotten and is related to the chemical composition of the filler metal.
So in ASME parameters related to chemistry and material properties are P, group, A number and indirectly the F number
Best regards
Dr Georgios Dilintas
Authorized Nuclear Inspector
Authorized Inspector Supervisor
HBS Regional Technical Manager


  From: Ammar Shaikh [ammar.ali.shaikh@gmail.com]
  Sent: 27/07/2012 20:34 ZE5
  To: materials-welding@googlegroups.com
  Subject: Re: [MW:14970] Need WPS clarification with ASME and EN


WPS for any specified material takes into consideration the chemical composition and mechanical properties which are validated by PQR.
You can use the WPS if chemical composition is within range, remember that a WPS is valid for all materials of same P No. 
I have used the same to successful results in a project. If you want you can get the same WPS validated by EN material PQR as an extra point for satisfaction.


Ammar Shaikh


On Thu, Jul 26, 2012 at 4:44 PM, c sridhar <sridhar305@yahoo.com> wrote:
yes,  U can use any ASME, IS, EN or any group if  P nos and Group nos  matches in all respects.

sridhar.


From: Vinayak Kale <Vinayak_Kale@Lntenc.com>
To: materials-welding@googlegroups.com
Sent: Thursday, 26 July 2012 8:36 AM
Subject: Re: [MW:14960] Need WPS clarification with ASME and EN


Can , provided , all essential parameters & properties shall match


Regards


Vinayak Kale
OGSP - QA & I , HC - Upstream
EPC Block , 2nd Floor , Gate No.1
Saki Vihar Rd. Powai Campus
Mumbai - 400072
Ph : + 91 022 6705 3969
(M) - 9987875309
www.larsen toubro.com



[MW:14959] Need WPS clarification with ASME and EN

Naresh Kumar  to:materials-welding@googlegroups.com
07/26/2012 08:34 AM

Sent by:materials-welding@googlegroups.com



From:Naresh Kumar <snareshkumar30@yahoo.com>
To:"materials-welding@googlegroups.com" <materials-welding@googlegroups.com>
Sent by:materials-welding@googlegroups.com
Please respond to materials-welding@googlegroups.com




Dear experts,

I have a doubt about WPS. Our company has WPS with ASTM material by ASME standard.
Whether this WPS can be used for the equivalent BS material or not.
 
 
Thanks & Regards,
Kumar S
--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at
http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.


Disclaimer :This email and any files transmitted with it are intended solely for the use of the addressee(s) only and may contain confidential and/or privileged information. If you are not the addressee, then this message is not intended for you and be advised that you have received this email in error and that any use , dissemination , forwarding, printing or copying of this email is strictly prohibited. In such case please notify the sender and delete this email and any attachments with it from your system immediately.Receipt of this email by you shall not give rise to any liability on the part of Larsen & Toubro Limited
--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.


--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~
NOTICE: This message contains information which is confidential and the copyright of our company or a third party. If you are not the intended recipient of this message please delete it and destroy all copies. If you
are the intended recipient of this message you should not disclose or distribute this message to third parties without the consent of our company. Our company does not represent, warrant and/or guarantee that the integrity of this message has been maintained nor that the communication is free of virus, interception or interference. The liability of our company is limited by our General Conditions of Services.
Nota : Ce message contient des informations confidentielles propriété de notre société et/ou d'un tiers. Si vous n'êtes pas parmi les destinataires désignés de ce message, merci de l'effacer ainsi que toutes ses copies. Si vous êtes parmi les destinataires désignés de ce message, prière de ne pas le divulguer ni de le transmettre à des tiers sans l'accord de notre société. Notre société ne peut garantir que l'intégrité de ce message a été préservée ni que la présente communication est sans virus, interception ou interférence. La responsabilité de notre société est limitée par nos Conditions Générales de Services.
~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...