Skip to main content

[MW:983] FW: 982] RE: 981] FW: 978] RE: 974] RE: 971] RE: 970] Consumable For UNS31254weldoverlay on SA516 Gr. 70

Sorry. The base material is UNS S31254 only.(typing error)

-----Original Message-----
From: materials-welding@googlegroups.com
[mailto:materials-welding@googlegroups.com] On Behalf Of Bathula Raghuram
(Mumbai - PIPING)
Sent: 29 July, 2008 9:10 AM
To: materials-welding@googlegroups.com
Subject: [MW:982] RE: 981] FW: 978] RE: 974] RE: 971] RE: 970] Consumable
For UNS31254weldoverlay on SA516 Gr. 70


Please note there is a difference in UNS# S32654 and UNS# S31524, you
are using 654SMO and the other one is 254SMO (what we are discussing
here)

-----Original Message-----
From: materials-welding@googlegroups.com
[mailto:materials-welding@googlegroups.com] On Behalf Of
mathu.subramanian
Sent: Tuesday, July 29, 2008 11:01 AM
To: materials-welding@googlegroups.com
Subject: [MW:981] FW: 978] RE: 974] RE: 971] RE: 970] Consumable For
UNS31254weldoverlay on SA516 Gr. 70


Dear Friends,

We are fabricating Evaporator Sump having base material of UNS S32654
for
the Canadian Vessel Manufacturer. With their recommendations only we are
using ENiCrMo-10.

Regards,

S.Mathusoothanan

-----Original Message-----
From: materials-welding@googlegroups.com
[mailto:materials-welding@googlegroups.com] On Behalf Of Abby Joseph
Sent: 29 July, 2008 6:51 AM
To: materials-welding@googlegroups.com
Subject: [MW:978] RE: 974] RE: 971] RE: 970] Consumable For UNS31254
weldoverlay on SA516 Gr. 70


Dear All,
Just to add further to this,
Avesta P12-R Basic (ENiCrMo-12) is best suited for welding UNS S31254.
The
Avesta P16 Basic electrode confirms to ENiCrMO-13 and is specifically
designed for welding 654SMO (UNS S32654) grades.

Regards,

Abby Joseph


-----Original Message-----
From: materials-welding@googlegroups.com
[mailto:materials-welding@googlegroups.com] On Behalf Of Bathula
Raghuram
(Mumbai - PIPING)
Sent: 28 July 2008 09:57
To: materials-welding@googlegroups.com
Subject: [MW:974] RE: 971] RE: 970] Consumable For UNS31254 weldoverlay
on
SA516 Gr. 70


UNS31254 is similar to Type 254SMO of Avesta polarit; you may contact
them for their recommended combination (Avesta P16 or P12-R basic etc.)
ERNiCrMo-3 (AWS Specification A5.14) or ENiCrMo-3/ ENiCrMo-12 (AWS
Specification A5.11) can be used for depositing, depending on the
process you may choose. E309LMo also can be used for barrier layer.
Avestapolarit has 805 flux which can be used in case of SAW

Sandvik also got similar combination such as Sanicro60 etc...

For strip cladding Soudokay has got some combinations, such as
Soudotape625 with flux NFT201/EST201 (refer their catalogue)


-----Original Message-----
From: materials-welding@googlegroups.com
[mailto:materials-welding@googlegroups.com] On Behalf Of
mathu.subramanian
Sent: Sunday, July 27, 2008 9:47 AM
To: materials-welding@googlegroups.com
Subject: [MW:971] RE: 970] Consumable For UNS31254 weldoverlay on SA516
Gr. 70

Dear Friend,

You can use ER NiCrMo-10.

Regards,

S.Mathusoothanan

-----Original Message-----
From: materials-welding@googlegroups.com
[mailto:materials-welding@googlegroups.com] On Behalf Of Romio
Sent: 26 July, 2008 3:15 PM
To: Materials & Welding
Subject: [MW:970] Consumable For UNS31254 weldoverlay on SA516 Gr. 70


Has anybody experienced UNS31254 (P No. 8 Gr. 4.....chemi..20Cr 18Ni
6Mo) weldoverlay on SA516 Gr. 70
Can someone suggest the correct AWS class? If u can suggest the STRIP
consumable supplier for the smae it will be handful....

Romio


--~--~---------~--~----~------------~-------~--~----~
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
-~----------~----~----~----~------~----~------~--~---

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Re: [MW:14950] RE: 14919] Stress relieving Rejected for 5 min less soaking time.

Dear All, I have been a CONSULTANT FOR such problem & my personal opinion is expressed as follow. I fully agree with views expressed so far. But bag to differ that " Code is a law, with engineering judgments. Hence the inspector has the rights to declare that the original HT was inadequate." Inspectors & total industry must resist the "REJECTION" . We as intellectual & having seniority must become practical. How the code will revise???. ANS.: One is experiments (Pure research) & second is such chances that gives opportunity to experiment !!! _______________________________________________________________________________________________ My understanding is that it is P1 material. In that case every pass normalizes the immediate bottom pass. Hence code requirement for P1 FOR MANDATORY SR is 32 mm & above thickness. SOLUTION:  In any case 0. After SR=PWHT no PTC testing is required as per code--Unless for low temp. vessels. That means code ...