[MW:974] RE: 971] RE: 970] Consumable For UNS31254 weldoverlay on SA516 Gr. 70

UNS31254 is similar to Type 254SMO of Avesta polarit; you may contact
them for their recommended combination (Avesta P16 or P12-R basic etc.)
ERNiCrMo-3 (AWS Specification A5.14) or ENiCrMo-3/ ENiCrMo-12 (AWS
Specification A5.11) can be used for depositing, depending on the
process you may choose. E309LMo also can be used for barrier layer.
Avestapolarit has 805 flux which can be used in case of SAW

Sandvik also got similar combination such as Sanicro60 etc...

For strip cladding Soudokay has got some combinations, such as
Soudotape625 with flux NFT201/EST201 (refer their catalogue)


-----Original Message-----
From: materials-welding@googlegroups.com
[mailto:materials-welding@googlegroups.com] On Behalf Of
mathu.subramanian
Sent: Sunday, July 27, 2008 9:47 AM
To: materials-welding@googlegroups.com
Subject: [MW:971] RE: 970] Consumable For UNS31254 weldoverlay on SA516
Gr. 70

Dear Friend,

You can use ER NiCrMo-10.

Regards,

S.Mathusoothanan

-----Original Message-----
From: materials-welding@googlegroups.com
[mailto:materials-welding@googlegroups.com] On Behalf Of Romio
Sent: 26 July, 2008 3:15 PM
To: Materials & Welding
Subject: [MW:970] Consumable For UNS31254 weldoverlay on SA516 Gr. 70


Has anybody experienced UNS31254 (P No. 8 Gr. 4.....chemi..20Cr 18Ni
6Mo) weldoverlay on SA516 Gr. 70
Can someone suggest the correct AWS class? If u can suggest the STRIP
consumable supplier for the smae it will be handful....

Romio

--~--~---------~--~----~------------~-------~--~----~
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
-~----------~----~----~----~------~----~------~--~---

No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...